Birches
Hardness among the 3 birches here ranges from 910 lbf (Paper birch) to 1,470 lbf (Sweet birch). The flattest-drying is Yellow birch; the stiffest is Sweet birch.
- None of the three has a T/R ratio above the median for all 155 woods (1.81).
- One of the three is in the hardest quarter of the 155 woods (1,465 lbf or more); the rest sit in the middle half.
- Density runs from a specific gravity of 0.48 in paper birch to 0.60 in sweet birch.
- The stiffest is sweet birch, at 2.17 million psi, 28th of all 155.
- 1,260 lbfmedian hardness
- 0.55median density
- 16,600 psimedian bending strength
- 9.0%median face shrinkage
BirchesOther woodsNorthern red oak, the usual yardstick
Ranked by hardness
Hardest first. Density is specific gravity; shrinkage is volumetric, green to oven-dry.
| # | Wood | Janka, lbf | Density | Bending, psi | Shrinkage |
|---|---|---|---|---|---|
| 1 | Sweet birchBetula lentaSG 0.60 · 15.6% shrinkage | 1,470 | 0.60 | 16,900 | 15.6% |
| 2 | Yellow birchBetula alleghaniensisSG 0.55 · 16.8% shrinkage | 1,260 | 0.55 | 16,600 | 16.8% |
| 3 | Paper birchBetula papyriferaSG 0.48 · 16.2% shrinkage | 910 | 0.48 | 12,300 | 16.2% |
Source: USDA Forest Products Laboratory, Wood Handbook (2010), Tables 4-3, 4-4, 5-3b and 5-5b. How we use the data · Compare or filter these woods · Guide: Hardwood vs softwood in numbers