Sugar maple
Acer saccharum
Sugar maple measures 1,450 lbf on the Janka scale, 12% harder than northern red oak.
- Of the five maples in the handbook, none is harder, heavier or stiffer, and none shrinks more across the face.
- Across all 155 woods it falls in the top fifth for face shrinkage.
- On the Janka scale its nearest neighbours are sepetir at 1,410 lbf and willow oak at 1,460 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Sugar mapleU.S. hardwoods medianOther woods
Shrinkage across the face
9.9%radial 4.8%23rd highest of 1553.5%12.7%Cupping tendency
2.0639th highest of 1551.092.90Janka hardness
1,450 lbf6,450 N41st hardest of 15510th of 53 U.S. hardwoods; 25% above the U.S. hardwoods median240 lbf3,680 lbfBending strength
15,800 psi108.9 MPa44th strongest of 1554,300 psi29,900 psiDensity
0.560.63 at 12% MC52nd heaviest of 1550.250.96Stiffness
1.83 M psi12.6 GPa53rd stiffest of 1550.54 M psi4.06 M psi
How much it moves
Most of its movement runs along the rings (T/R 2.06): quartersawn, the same board would lose 0.29 in. instead of 0.59 in.
0.59 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 9.9%
- Radial
- 4.8%
- Volume
- 14.7%
- T/R ratio
- 2.06 (117th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Willow oak
1% harder · same density · shrinks 0.3 points less across the face
- Water oak
18% softer · same density · shrinks 0.1 points less across the face
- Pin oak
4% harder · 4% heavier · shrinks 0.4 points less across the face
Among the maples
1st hardest of 5, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: 7th highest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 640psi | 1,470psi | +130% | 10.1MPa |
| Shear parallel to grain | 1,460psi | 2,330psi | +60% | 16.1MPa |
| Work to maximum load | 13.3in-lbf/in³ | 16.5in-lbf/in³ | +24% | 113.8kJ/m³ |
| Side hardness | 970lbf | 1,450lbf | +49% | 6,450N |
| Impact bending | 40in. | 39in. | −2% | 991mm |
| Modulus of rupture | 9,400psi | 15,800psi | +68% | 108.9MPa |
| Compression parallel to grain | 4,020psi | 7,830psi | +95% | 54MPa |
| Modulus of elasticity | 1.55M psi | 1.83M psi | +18% | 12.6GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides