Green ash
Fraxinus pennsylvanica
Green ash measures 1,200 lbf on the Janka scale, 7% softer than northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Green ashU.S. hardwoods medianOther woods
Cupping tendency
1.5429th lowest of 1551.092.90Shrinkage across the face
7.1%radial 4.6%48th lowest of 1553.5%12.7%Janka hardness
1,200 lbf5,338 N62nd hardest of 15523rd of 53 U.S. hardwoods240 lbf3,680 lbfBending strength
14,100 psi97.2 MPa62nd strongest of 1554,300 psi29,900 psiDensity
0.530.56 at 12% MC68th heaviest of 1550.250.96Stiffness
1.66 M psi11.4 GPa75th stiffest of 1550.54 M psi4.06 M psi
How much it moves
The two directions move almost alike (T/R 1.54), so flatsawn and quartersawn boards differ by only 0.15 in.
0.43 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 7.1%
- Radial
- 4.6%
- Volume
- 12.5%
- T/R ratio
- 1.54 (29th most stable of 155)
End view, shrinkage drawn 3× life size.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: 9th highest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 730psi | 1,310psi | +79% | 9.00MPa |
| Tension perpendicular | 590psi | 700psi | +19% | 4.80MPa |
| Shear parallel to grain | 1,260psi | 1,910psi | +52% | 13.2MPa |
| Work to maximum load | 11.8in-lbf/in³ | 13.4in-lbf/in³ | +14% | 92.4kJ/m³ |
| Modulus of rupture | 9,500psi | 14,100psi | +48% | 97.2MPa |
| Side hardness | 870lbf | 1,200lbf | +38% | 5,338N |
| Impact bending | 35in. | 32in. | −9% | 813mm |
| Compression parallel to grain | 4,200psi | 7,080psi | +69% | 48.8MPa |
| Modulus of elasticity | 1.40M psi | 1.66M psi | +19% | 11.4GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides