Manbarklak
Eschweilera spp.
Manbarklak measures 3,480 lbf on the Janka scale, 170% harder than northern red oak.
- Only ipe and marishballi are harder, and only four woods are heavier, four stronger in bending and five stiffer.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
ManbarklakImported woods medianOther woods
Janka hardness
3,480 lbf15,480 N3rd hardest of 1553rd of 65 imported woods; 168% above the imported woods median240 lbf3,680 lbfDensity
0.875th heaviest of 15543% above the imported woods median0.250.96Bending strength
26,500 psi182.7 MPa5th strongest of 15559% above the imported woods median4,300 psi29,900 psiStiffness
3.14 M psi21.6 GPa6th stiffest of 15557% above the imported woods median0.54 M psi4.06 M psiShrinkage across the face
10.3%radial 5.8%20th highest of 15530% above the imported woods median3.5%12.7%Cupping tendency
1.7870th lowest of 1551.092.90
For its weight: strength-to-weight 30,460 psi (12th of 155).
How much it moves
Its face shrinkage of 10.3% is in the top quarter of the list, with an ordinary T/R ratio of 1.78.
0.62 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.35 in.
- Tangential
- 10.3%
- Radial
- 5.8%
- Volume
- 15.9%
- T/R ratio
- 1.78 (70th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Bulletwood
8% softer · 2% lighter · shrinks 0.9 points less across the face
- Ipe
6% harder · 6% heavier · shrinks 2.3 points less across the face
- Tropical oak (roble)
28% softer · 13% lighter · shrinks 1.4 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is work to maximum load: the highest of the 142 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 17.4in-lbf/in³ | 33.3in-lbf/in³ | +91% | 229.6kJ/m³ |
| Side hardness | 2,280lbf | 3,480lbf | +53% | 15,480N |
| Modulus of rupture | 17,100psi | 26,500psi | +55% | 182.7MPa |
| Modulus of elasticity | 2.70M psi | 3.14M psi | +16% | 21.6GPa |
| Compression parallel to grain | 7,340psi | 11,210psi | +53% | 77.3MPa |
| Shear parallel to grain | 1,630psi | 2,070psi | +27% | 14.3MPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides