American basswood
Tilia americana
American basswood measures 410 lbf on the Janka scale, about 32% as hard as northern red oak.
- Of the 155 woods, only four are stiffer for their weight and eight lighter.
- Soft as it is, it moves a lot: in the softest quarter of the list, but in the top quarter for shrinkage across the face.
- Drying hardens it more than most: from 250 lbf green, it gains 64% by 12% moisture, where the median wood gains 31%.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
American basswoodU.S. hardwoods medianOther woods
Density
0.320.37 at 12% MC9th lightest of 15538% below the U.S. hardwoods median0.250.96Janka hardness
410 lbf1,824 N14th softest of 15551st of 53 U.S. hardwoods; 65% below the U.S. hardwoods median240 lbf3,680 lbfCupping tendency
1.4114th lowest of 15525% below the U.S. hardwoods median1.092.90Bending strength
8,700 psi60.0 MPa19th weakest of 15533% below the U.S. hardwoods median4,300 psi29,900 psiShrinkage across the face
9.3%radial 6.6%37th highest of 1553.5%12.7%Stiffness
1.46 M psi10.1 GPa45th most flexible of 1550.54 M psi4.06 M psi
For its weight: stiffness-to-weight 4.56 (5th of 155).
How much it moves
It shrinks a lot, but the two directions stay close (T/R 1.41), so a board loses size more than it changes shape.
0.56 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.40 in.
- Tangential
- 9.3%
- Radial
- 6.6%
- Volume
- 15.8%
- T/R ratio
- 1.41 (14th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Light red meranti
12% harder · 6% heavier · shrinks 0.8 points less across the face
- Yellow-poplar
32% harder · 25% heavier · shrinks 1.1 points less across the face
- Ilomba
49% harder · 25% heavier · shrinks 0.9 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: 3rd lowest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 170psi | 370psi | +118% | 2.60MPa |
| Impact bending | 16in. | 16in. | ±0% | 406mm |
| Compression parallel to grain | 2,220psi | 4,730psi | +113% | 32.6MPa |
| Side hardness | 250lbf | 410lbf | +64% | 1,824N |
| Shear parallel to grain | 600psi | 990psi | +65% | 6.80MPa |
| Modulus of rupture | 5,000psi | 8,700psi | +74% | 60MPa |
| Work to maximum load | 5.30in-lbf/in³ | 7.20in-lbf/in³ | +36% | 49.6kJ/m³ |
| Tension perpendicular | 280psi | 350psi | +25% | 2.40MPa |
| Modulus of elasticity | 1.04M psi | 1.46M psi | +40% | 10.1GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides