Slippery elm
Ulmus rubra
Slippery elm measures 860 lbf on the Janka scale, 33% softer than northern red oak.
- On the Janka scale its nearest neighbours are sweetgum at 850 lbf and longleaf pine at 870 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Slippery elmU.S. hardwoods medianOther woods
Shrinkage across the face
8.9%radial 4.9%44th highest of 1553.5%12.7%Stiffness
1.49 M psi10.3 GPa48th most flexible of 1550.54 M psi4.06 M psiJanka hardness
860 lbf3,825 N71st softest of 15537th of 53 U.S. hardwoods; 26% below the U.S. hardwoods median240 lbf3,680 lbfDensity
0.480.53 at 12% MC71st lightest of 1550.250.96Bending strength
13,000 psi89.6 MPa75th strongest of 1554,300 psi29,900 psiCupping tendency
1.8276th highest of 1551.092.90
How much it moves
Both its face shrinkage (8.9%) and its T/R ratio (1.82) sit in the middle half of the list.
0.53 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.29 in.
- Tangential
- 8.9%
- Radial
- 4.9%
- Volume
- 13.8%
- T/R ratio
- 1.82 (79th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Black ash
1% softer · 6% lighter · shrinks 1.1 points less across the face
- Black maple
37% harder · 8% heavier · shrinks 0.4 points more across the face
- Hackberry
2% harder · 2% heavier · same face shrinkage
Among the elms
2nd hardest of 3, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Impact bending | 47in. | 45in. | −4% | 1,143mm |
| Work to maximum load | 15.4in-lbf/in³ | 16.9in-lbf/in³ | +10% | 116.5kJ/m³ |
| Modulus of elasticity | 1.23M psi | 1.49M psi | +21% | 10.3GPa |
| Compression parallel to grain | 3,320psi | 6,360psi | +92% | 43.9MPa |
| Compression perpendicular | 420psi | 820psi | +95% | 5.70MPa |
| Tension perpendicular | 640psi | 530psi | −17% | 3.70MPa |
| Side hardness | 660lbf | 860lbf | +30% | 3,825N |
| Shear parallel to grain | 1,110psi | 1,630psi | +47% | 11.2MPa |
| Modulus of rupture | 8,000psi | 13,000psi | +62% | 89.6MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides