Southern magnolia
Magnolia grandiflora
Southern magnolia measures 1,020 lbf on the Janka scale, 21% softer than northern red oak.
- Only greenheart and ipe have a T/R ratio closer to 1.
- Among the 53 U.S. hardwoods, only butternut shrinks less across the face.
- Albarco has exactly the same Janka figure.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Southern magnoliaU.S. hardwoods medianOther woods
Cupping tendency
1.223rd lowest of 15535% below the U.S. hardwoods median1.092.90Shrinkage across the face
6.6%radial 5.4%32nd lowest of 15526% below the U.S. hardwoods median3.5%12.7%Stiffness
1.40 M psi9.7 GPa37th most flexible of 1550.54 M psi4.06 M psiBending strength
11,200 psi77.2 MPa55th weakest of 1554,300 psi29,900 psiDensity
0.460.50 at 12% MC58th lightest of 1550.250.96Janka hardness
1,020 lbf4,537 N72nd hardest of 15530th of 53 U.S. hardwoods240 lbf3,680 lbf
How much it moves
Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.
0.40 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.32 in.
- Tangential
- 6.6%
- Radial
- 5.4%
- Volume
- 12.3%
- T/R ratio
- 1.22 (3rd most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Avodire
6% harder · 4% heavier · shrinks 0.1 points more across the face
- Black ash
17% softer · 2% lighter · shrinks 1.2 points more across the face
- American sycamore
24% softer · same density · shrinks 1.8 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Tension perpendicular | 610psi | 740psi | +21% | 5.10MPa |
| Compression parallel to grain | 2,700psi | 5,460psi | +102% | 37.6MPa |
| Modulus of elasticity | 1.11M psi | 1.40M psi | +26% | 9.65GPa |
| Modulus of rupture | 6,800psi | 11,200psi | +65% | 77.2MPa |
| Compression perpendicular | 460psi | 860psi | +87% | 5.90MPa |
| Work to maximum load | 15.4in-lbf/in³ | 12.8in-lbf/in³ | −17% | 88.3kJ/m³ |
| Side hardness | 740lbf | 1,020lbf | +38% | 4,537N |
| Impact bending | 54in. | 29in. | −46% | 737mm |
| Shear parallel to grain | 1,040psi | 1,530psi | +47% | 10.5MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides