Angelin
Andira inermis
Angelin measures 1,750 lbf on the Janka scale, 36% harder than northern red oak.
- Of the 14 woods from Africa in the tables, none is stiffer.
- It sits in the top quarter of the list for both hardness and shrinkage across the face.
- Benge has exactly the same Janka figure.
- Across all 155 woods it falls in the top fifth for hardness, density, bending strength, stiffness, face shrinkage and T/R ratio.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
AngelinImported woods medianOther woods
Stiffness
2.49 M psi17.2 GPa13th stiffest of 1550.54 M psi4.06 M psiJanka hardness
1,750 lbf7,784 N25th hardest of 15521st of 65 imported woods; 35% above the imported woods median240 lbf3,680 lbfShrinkage across the face
9.8%radial 4.6%25th highest of 1553.5%12.7%Density
0.6528th heaviest of 1550.250.96Bending strength
18,000 psi124.1 MPa29th strongest of 1554,300 psi29,900 psiCupping tendency
2.1331st highest of 1551.092.90
How much it moves
Most of its movement runs along the rings (T/R 2.13): quartersawn, the same board would lose 0.28 in. instead of 0.59 in.
0.59 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 9.8%
- Radial
- 4.6%
- Volume
- 12.5%
- T/R ratio
- 2.13 (124th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is stiffness (modulus of elasticity): 13th highest of the 155 woods with a published value.
| Property | Dry, 12% MC | Metric, 12% MC |
|---|---|---|
| Modulus of elasticity | 2.49M psi | 17.2GPa |
| Side hardness | 1,750lbf | 7,784N |
| Modulus of rupture | 18,000psi | 124.1MPa |
| Compression parallel to grain | 9,200psi | 63.4MPa |
| Shear parallel to grain | 1,840psi | 12.7MPa |
The handbook publishes only values at 12% moisture content for this wood; green values and some tests are not given.
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides