Butternut
Juglans cinerea
Butternut measures 490 lbf on the Janka scale, about 38% as hard as northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
ButternutU.S. hardwoods medianOther woods
Bending strength
8,100 psi55.8 MPa10th weakest of 15538% below the U.S. hardwoods median4,300 psi29,900 psiStiffness
1.18 M psi8.1 GPa15th most flexible of 15526% below the U.S. hardwoods median0.54 M psi4.06 M psiDensity
0.360.38 at 12% MC21st lightest of 15531% below the U.S. hardwoods median0.250.96Janka hardness
490 lbf2,180 N27th softest of 15549th of 53 U.S. hardwoods; 58% below the U.S. hardwoods median240 lbf3,680 lbfShrinkage across the face
6.4%radial 3.4%29th lowest of 15528% below the U.S. hardwoods median3.5%12.7%Cupping tendency
1.8866th highest of 1551.092.90
For its weight: strength-to-weight 22,500 psi (136th of 155).
How much it moves
Its face shrinkage of 6.4% is in the lowest quarter of the list, with an ordinary T/R ratio of 1.88.
0.38 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.20 in.
- Tangential
- 6.4%
- Radial
- 3.4%
- Volume
- 10.6%
- T/R ratio
- 1.88 (89th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- American chestnut
10% harder · 11% heavier · shrinks 0.3 points more across the face
- Quaking aspen
29% softer · 3% lighter · shrinks 0.3 points more across the face
- Okoume
22% softer · 8% lighter · shrinks 0.3 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is bending strength (modulus of rupture): 10th lowest of the 155 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Modulus of rupture | 5,400psi | 8,100psi | +50% | 55.8MPa |
| Modulus of elasticity | 0.97M psi | 1.18M psi | +22% | 8.14GPa |
| Compression parallel to grain | 2,420psi | 5,110psi | +111% | 35.2MPa |
| Compression perpendicular | 220psi | 460psi | +109% | 3.20MPa |
| Side hardness | 390lbf | 490lbf | +26% | 2,180N |
| Work to maximum load | 8.20in-lbf/in³ | 8.20in-lbf/in³ | ±0% | 56.5kJ/m³ |
| Shear parallel to grain | 760psi | 1,170psi | +54% | 8.10MPa |
| Impact bending | 24in. | 24in. | ±0% | 610mm |
| Tension perpendicular | 430psi | 440psi | +2% | 3.00MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides