Water tupelo
Nyssa aquatica
Water tupelo measures 880 lbf on the Janka scale, 32% softer than northern red oak.
- Hackberry has exactly the same Janka figure.
- Across all 155 woods it falls in the bottom fifth for bending strength and stiffness.
- On the Janka scale its nearest neighbours are longleaf pine at 870 lbf and sande at 900 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Water tupeloU.S. hardwoods medianOther woods
Stiffness
1.26 M psi8.7 GPa24th most flexible of 1550.54 M psi4.06 M psiBending strength
9,600 psi66.2 MPa31st weakest of 15526% below the U.S. hardwoods median4,300 psi29,900 psiDensity
0.460.50 at 12% MC58th lightest of 1550.250.96Shrinkage across the face
7.6%radial 4.2%70th lowest of 1553.5%12.7%Janka hardness
880 lbf3,914 N73rd softest of 15535th of 53 U.S. hardwoods240 lbf3,680 lbfCupping tendency
1.8177th lowest of 1551.092.90
For its weight: stiffness-to-weight 2.74 (138th of 155); strength-to-weight 20,870 psi (148th of 155).
How much it moves
Both its face shrinkage (7.6%) and its T/R ratio (1.81) sit in the middle half of the list.
0.46 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.25 in.
- Tangential
- 7.6%
- Radial
- 4.2%
- Volume
- 12.5%
- T/R ratio
- 1.81 (77th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Bigleaf maple
3% softer · 4% lighter · shrinks 0.5 points less across the face
- American sycamore
12% softer · same density · shrinks 0.8 points more across the face
- Black cherry
8% harder · 2% heavier · shrinks 0.5 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 8.30in-lbf/in³ | 6.90in-lbf/in³ | −17% | 47.6kJ/m³ |
| Modulus of elasticity | 1.05M psi | 1.26M psi | +20% | 8.69GPa |
| Modulus of rupture | 7,300psi | 9,600psi | +32% | 66.2MPa |
| Tension perpendicular | 600psi | 700psi | +17% | 4.80MPa |
| Impact bending | 30in. | 23in. | −23% | 584mm |
| Compression parallel to grain | 3,370psi | 5,920psi | +76% | 40.8MPa |
| Compression perpendicular | 480psi | 870psi | +81% | 6.00MPa |
| Side hardness | 710lbf | 880lbf | +24% | 3,914N |
| Shear parallel to grain | 1,190psi | 1,590psi | +34% | 11MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides