Sande
Brosimum spp. (utile group)
Sande measures 900 lbf on the Janka scale, 30% softer than northern red oak.
- Only cuangare is stiffer for its weight.
- Across all 155 woods it falls in the top fifth for stiffness.
- On the Janka scale its nearest neighbours are water tupelo at 880 lbf and ocote pine at 910 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
SandeImported woods medianOther woods
Stiffness
2.39 M psi16.5 GPa17th stiffest of 1550.54 M psi4.06 M psiBending strength
14,300 psi98.6 MPa60th strongest of 1554,300 psi29,900 psiCupping tendency
1.7466th lowest of 1551.092.90Shrinkage across the face
8.0%radial 4.6%68th highest of 1553.5%12.7%Janka hardness
900 lbf4,003 N75th softest of 15547th of 65 imported woods; 31% below the imported woods median240 lbf3,680 lbfDensity
0.4976th lightest of 1550.250.96
For its weight: stiffness-to-weight 4.88 (2nd of 155).
How much it moves
Both its face shrinkage (8.0%) and its T/R ratio (1.74) sit in the middle half of the list.
0.48 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.28 in.
- Tangential
- 8.0%
- Radial
- 4.6%
- Volume
- 13.6%
- T/R ratio
- 1.74 (66th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Modulus of elasticity | 1.94M psi | 2.39M psi | +23% | 16.5GPa |
| Compression parallel to grain | 4,490psi | 8,220psi | +83% | 56.7MPa |
| Shear parallel to grain | 1,040psi | 1,290psi | +24% | 8.90MPa |
| Modulus of rupture | 8,500psi | 14,300psi | +68% | 98.6MPa |
| Side hardness | 600lbf | 900lbf | +50% | 4,003N |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides