Primavera
Tabebuia donnell-smithii
Primavera measures 660 lbf on the Janka scale, 49% softer than northern red oak.
- Of the three Tabebuia (ipe, roble, primavera) in the handbook, none is softer or lighter, and none shrinks less across the face.
- Only six of the 155 woods bend more easily.
- Unusually, it tests harder green (700 lbf) than dry.
- Its stiffness is 48% below the median for imported woods.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
PrimaveraImported woods medianOther woods
Stiffness
1.04 M psi7.2 GPa7th most flexible of 15548% below the imported woods median0.54 M psi4.06 M psiShrinkage across the face
5.1%radial 3.1%12th lowest of 15535% below the imported woods median3.5%12.7%Bending strength
9,500 psi65.5 MPa29th weakest of 15543% below the imported woods median4,300 psi29,900 psiDensity
0.4036th lightest of 15534% below the imported woods median0.250.96Janka hardness
660 lbf2,936 N49th softest of 15553rd of 65 imported woods; 49% below the imported woods median240 lbf3,680 lbfCupping tendency
1.6549th lowest of 1551.092.90
For its weight: stiffness-to-weight 2.60 (146th of 155).
How much it moves
Its face shrinkage of 5.1% is in the lowest quarter of the list, with an ordinary T/R ratio of 1.65.
0.31 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.19 in.
- Tangential
- 5.1%
- Radial
- 3.1%
- Volume
- 9.1%
- T/R ratio
- 1.65 (49th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Cativo
4% softer · same density · shrinks 0.2 points more across the face
- Hura
17% softer · 5% lighter · shrinks 0.6 points less across the face
- African mahogany
26% harder · 5% heavier · shrinks 0.6 points less across the face
Among the Tabebuia (ipe, roble, primavera)
3rd hardest of 3, lbf.
Laboratory values
Its most unusual laboratory figure is stiffness (modulus of elasticity): 7th lowest of the 155 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Modulus of elasticity | 0.99M psi | 1.04M psi | +5% | 7.17GPa |
| Work to maximum load | 7.20in-lbf/in³ | 6.40in-lbf/in³ | −11% | 44.1kJ/m³ |
| Modulus of rupture | 7,200psi | 9,500psi | +32% | 65.5MPa |
| Compression parallel to grain | 3,510psi | 5,600psi | +60% | 38.6MPa |
| Side hardness | 700lbf | 660lbf | −6% | 2,936N |
| Shear parallel to grain | 1,030psi | 1,390psi | +35% | 9.60MPa |
Note on the data: the published side hardness at 12% MC is lower than the green value.
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides