Post oak
Quercus stellata
Post oak measures 1,360 lbf on the Janka scale, 5% harder than northern red oak.
- Of the 15 oaks in the handbook, none has a T/R ratio closer to 1.
- White oak has exactly the same Janka figure.
- Across all 155 woods it falls in the top fifth for face shrinkage, radial shrinkage and volumetric shrinkage.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Post oakU.S. hardwoods medianOther woods
Shrinkage across the face
9.8%radial 5.4%25th highest of 1553.5%12.7%Density
0.600.67 at 12% MC39th heaviest of 1550.250.96Janka hardness
1,360 lbf6,050 N45th hardest of 15513th of 53 U.S. hardwoods240 lbf3,680 lbfStiffness
1.51 M psi10.4 GPa56th most flexible of 1550.54 M psi4.06 M psiBending strength
13,200 psi91.0 MPa72nd strongest of 1554,300 psi29,900 psiCupping tendency
1.8177th lowest of 1551.092.90
For its weight: stiffness-to-weight 2.52 (148th of 155); strength-to-weight 22,000 psi (142nd of 155).
How much it moves
Its face shrinkage of 9.8% is in the top quarter of the list, with an ordinary T/R ratio of 1.81.
0.59 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.32 in.
- Tangential
- 9.8%
- Radial
- 5.4%
- Volume
- 16.2%
- T/R ratio
- 1.81 (77th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Chestnut oak
17% softer · 5% lighter · shrinks 1.0 points more across the face
- Swamp chestnut oak
9% softer · same density · shrinks 1.0 points more across the face
- White oak
Same hardness · same density · shrinks 0.7 points more across the face
Among the oaks
6th hardest of 15, lbf; the neighbours either side are shown, the rest are on the oaks page.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: 8th highest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 860psi | 1,430psi | +66% | 9.90MPa |
| Impact bending | 44in. | 46in. | +5% | 1,168mm |
| Tension perpendicular | 790psi | 780psi | −1% | 5.40MPa |
| Side hardness | 1,130lbf | 1,360lbf | +20% | 6,050N |
| Shear parallel to grain | 1,280psi | 1,840psi | +44% | 12.7MPa |
| Modulus of elasticity | 1.09M psi | 1.51M psi | +39% | 10.4GPa |
| Work to maximum load | 11in-lbf/in³ | 13.2in-lbf/in³ | +20% | 91kJ/m³ |
| Compression parallel to grain | 3,480psi | 6,600psi | +90% | 45.5MPa |
| Modulus of rupture | 8,100psi | 13,200psi | +63% | 91MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides