Roble
Tabebuia spp. (roble group)
Roble measures 960 lbf on the Janka scale, 26% softer than northern red oak.
- Of the three Tabebuia (ipe, roble, primavera) in the handbook, none has a higher T/R ratio.
- Drying barely changes its hardness: from 910 lbf green, it gains only 5% by 12% moisture, against a median of 31%.
- Across all 155 woods it falls in the bottom fifth for face shrinkage and volumetric shrinkage.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
RobleImported woods medianOther woods
Shrinkage across the face
6.1%radial 3.6%22nd lowest of 1553.5%12.7%Cupping tendency
1.6958th lowest of 1551.092.90Bending strength
13,800 psi95.1 MPa66th strongest of 1554,300 psi29,900 psiDensity
0.5269th heaviest of 1550.250.96Stiffness
1.60 M psi11.0 GPa69th most flexible of 1550.54 M psi4.06 M psiJanka hardness
960 lbf4,270 N76th hardest of 15545th of 65 imported woods; 26% below the imported woods median240 lbf3,680 lbf
How much it moves
Its face shrinkage of 6.1% is in the lowest quarter of the list, with an ordinary T/R ratio of 1.69.
0.37 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.22 in.
- Tangential
- 6.1%
- Radial
- 3.6%
- Volume
- 9.5%
- T/R ratio
- 1.69 (58th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Black cherry
1% softer · 10% lighter · shrinks 1.0 points more across the face
- Albarco
6% harder · 8% lighter · shrinks 0.7 points less across the face
- Teak
4% harder · 6% heavier · shrinks 0.3 points less across the face
Among the Tabebuia (ipe, roble, primavera)
2nd hardest of 3, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression parallel to grain | 4,910psi | 7,340psi | +49% | 50.6MPa |
| Modulus of rupture | 10,800psi | 13,800psi | +28% | 95.1MPa |
| Shear parallel to grain | 1,250psi | 1,450psi | +16% | 10MPa |
| Work to maximum load | 11.7in-lbf/in³ | 12.5in-lbf/in³ | +7% | 86.2kJ/m³ |
| Modulus of elasticity | 1.45M psi | 1.60M psi | +10% | 11.0GPa |
| Side hardness | 910lbf | 960lbf | +5% | 4,270N |