Ramin
Gonystylus bancanus
Ramin measures 1,300 lbf on the Janka scale, 1% harder than northern red oak.
- No other wood in the tables is stronger for its weight.
- Drying hardens it more than most: from 640 lbf green, it gains 103% by 12% moisture, where the median wood gains 31%.
- American beech has exactly the same Janka figure.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
RaminImported woods medianOther woods
Bending strength
18,500 psi127.6 MPa24th strongest of 1554,300 psi29,900 psiStiffness
2.17 M psi15.0 GPa28th stiffest of 1550.54 M psi4.06 M psiCupping tendency
2.0243rd highest of 1551.092.90Janka hardness
1,300 lbf5,783 N49th hardest of 15533rd of 65 imported woods240 lbf3,680 lbfShrinkage across the face
8.7%radial 4.3%50th highest of 1553.5%12.7%Density
0.5269th heaviest of 1550.250.96
For its weight: stiffness-to-weight 4.17 (16th of 155); strength-to-weight 35,577 psi (1st of 155).
How much it moves
Both its face shrinkage (8.7%) and its T/R ratio (2.02) sit in the middle half of the list.
0.52 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.26 in.
- Tangential
- 8.7%
- Radial
- 4.3%
- Volume
- 13.4%
- T/R ratio
- 2.02 (112th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression parallel to grain | 5,390psi | 10,080psi | +87% | 69.5MPa |
| Modulus of rupture | 9,800psi | 18,500psi | +89% | 127.6MPa |
| Work to maximum load | 9.00in-lbf/in³ | 17in-lbf/in³ | +89% | 117.2kJ/m³ |
| Modulus of elasticity | 1.57M psi | 2.17M psi | +38% | 15.0GPa |
| Side hardness | 640lbf | 1,300lbf | +103% | 5,783N |
| Shear parallel to grain | 990psi | 1,520psi | +54% | 10.5MPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides