Greenheart
Chlorocardium rodiei
Greenheart measures 2,350 lbf on the Janka scale, 82% harder than northern red oak.
- No other wood in the tables has a T/R ratio closer to 1 or shrinks more through the thickness.
- Only kaneelhart, bulletwood and marishballi are stiffer, and only six woods are stronger in bending.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
GreenheartImported woods medianOther woods
Cupping tendency
1.091st lowest of 15537% below the imported woods median1.092.90Stiffness
3.25 M psi22.4 GPa4th stiffest of 15562% above the imported woods median0.54 M psi4.06 M psiBending strength
24,900 psi171.7 MPa7th strongest of 15549% above the imported woods median4,300 psi29,900 psiDensity
0.8010th heaviest of 15531% above the imported woods median0.250.96Janka hardness
2,350 lbf10,453 N12th hardest of 15512th of 65 imported woods; 81% above the imported woods median240 lbf3,680 lbfShrinkage across the face
9.6%radial 8.8%30th highest of 1553.5%12.7%
For its weight: strength-to-weight 31,125 psi (10th of 155).
How much it moves
It shrinks a lot, but the two directions stay close (T/R 1.09), so a board loses size more than it changes shape.
0.58 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.53 in.
- Tangential
- 9.6%
- Radial
- 8.8%
- Volume
- 17.1%
- T/R ratio
- 1.09 (1st most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Mora
2% softer · 2% lighter · shrinks 0.2 points more across the face
- Azobe
43% harder · 9% heavier · shrinks 1.4 points more across the face
- Marishballi
52% harder · 10% heavier · shrinks 2.1 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is shear strength: 3rd highest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Shear parallel to grain | 1,930psi | 2,620psi | +36% | 18.1MPa |
| Modulus of elasticity | 2.47M psi | 3.25M psi | +32% | 22.4GPa |
| Compression parallel to grain | 9,380psi | 12,510psi | +33% | 86.3MPa |
| Modulus of rupture | 19,300psi | 24,900psi | +29% | 171.7MPa |
| Work to maximum load | 10.5in-lbf/in³ | 25.3in-lbf/in³ | +141% | 174.4kJ/m³ |
| Side hardness | 1,880lbf | 2,350lbf | +25% | 10,453N |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides