Mora measures 2,300 lbf on the Janka scale, 78% harder than northern red oak.
- Of the 155 woods, only four lose more volume on drying and eight are stiffer.
- It sits in the top quarter of the list for both hardness and shrinkage across the face.
- Drying hardens it more than most: from 1,450 lbf green, it gains 59% by 12% moisture, where the median wood gains 31%.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
MoraImported woods medianOther woods
Stiffness
2.96 M psi20.4 GPa9th stiffest of 15548% above the imported woods median0.54 M psi4.06 M psiDensity
0.7812th heaviest of 15528% above the imported woods median0.250.96Bending strength
22,100 psi152.4 MPa12th strongest of 15532% above the imported woods median4,300 psi29,900 psiJanka hardness
2,300 lbf10,231 N14th hardest of 15514th of 65 imported woods; 77% above the imported woods median240 lbf3,680 lbfCupping tendency
1.4215th lowest of 1551.092.90Shrinkage across the face
9.8%radial 6.9%25th highest of 1553.5%12.7%
How much it moves
It shrinks a lot, but the two directions stay close (T/R 1.42), so a board loses size more than it changes shape.
0.59 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.41 in.
- Tangential
- 9.8%
- Radial
- 6.9%
- Volume
- 18.8%
- T/R ratio
- 1.42 (15th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Tropical oak (roble)
9% harder · 3% lighter · shrinks 1.9 points more across the face
- Bubinga
17% harder · 9% lighter · shrinks 1.4 points less across the face
- Manbarklak
51% harder · 12% heavier · shrinks 0.5 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength along the grain: 8th highest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression parallel to grain | 6,400psi | 11,840psi | +85% | 81.6MPa |
| Modulus of elasticity | 2.33M psi | 2.96M psi | +27% | 20.4GPa |
| Modulus of rupture | 12,600psi | 22,100psi | +75% | 152.4MPa |
| Side hardness | 1,450lbf | 2,300lbf | +59% | 10,231N |
| Work to maximum load | 13.5in-lbf/in³ | 18.5in-lbf/in³ | +37% | 127.6kJ/m³ |
| Shear parallel to grain | 1,400psi | 1,900psi | +36% | 13.1MPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides