Western redcedar
Thuja plicata
Western redcedar measures 350 lbf on the Janka scale, about 27% as hard as northern red oak.
- Only macawood loses less volume on drying, only ceiba and northern white-cedar are softer, only ceiba, northern white-cedar and obeche are lighter, and only four woods shrink less through the thickness.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Western redcedarU.S. softwoods medianOther woods
Janka hardness
350 lbf1,557 N3rd softest of 15534th of 37 U.S. softwoods; 30% below the U.S. softwoods median240 lbf3,680 lbfDensity
0.310.32 at 12% MC4th lightest of 1550.250.96Bending strength
7,500 psi51.7 MPa7th weakest of 15526% below the U.S. softwoods median4,300 psi29,900 psiStiffness
1.11 M psi7.7 GPa10th most flexible of 15526% below the U.S. softwoods median0.54 M psi4.06 M psiShrinkage across the face
5.0%radial 2.4%11th lowest of 15530% below the U.S. softwoods median3.5%12.7%Cupping tendency
2.0836th highest of 1551.092.90
How much it moves
Total movement is small, but most of it runs along the rings (T/R 2.08), so a flatsawn board still loses 2.1 times the width of a quartersawn one.
0.30 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.14 in.
- Tangential
- 5.0%
- Radial
- 2.4%
- Volume
- 6.8%
- T/R ratio
- 2.08 (118th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Redwood (young-growth)
20% harder · 10% heavier · shrinks 0.1 points less across the face
- Atlantic white-cedar
Same hardness · same density · shrinks 0.4 points more across the face
- Sugar pine
9% harder · 10% heavier · shrinks 0.6 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is tension across the grain: 2nd lowest of the 73 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Side hardness | 260lbf | 350lbf | +35% | 1,557N |
| Tension perpendicular | 230psi | 220psi | −4% | 1.50MPa |
| Modulus of rupture | 5,200psi | 7,500psi | +44% | 51.7MPa |
| Impact bending | 17in. | 17in. | ±0% | 432mm |
| Work to maximum load | 5.00in-lbf/in³ | 5.80in-lbf/in³ | +16% | 40kJ/m³ |
| Modulus of elasticity | 0.94M psi | 1.11M psi | +18% | 7.65GPa |
| Compression parallel to grain | 2,770psi | 4,560psi | +65% | 31.4MPa |
| Shear parallel to grain | 770psi | 990psi | +29% | 6.80MPa |
| Compression perpendicular | 240psi | 460psi | +92% | 3.20MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides