Black cottonwood
Populus trichocarpa
Black cottonwood measures 350 lbf on the Janka scale, about 27% as hard as northern red oak.
- Only ceiba and northern white-cedar are softer, only ceiba, northern white-cedar and obeche are lighter, and only nine woods have a higher T/R ratio.
- Four other woods share exactly the same Janka figure.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Black cottonwoodU.S. hardwoods medianOther woods
Janka hardness
350 lbf1,557 N3rd softest of 15552nd of 53 U.S. hardwoods; 70% below the U.S. hardwoods median240 lbf3,680 lbfDensity
0.310.35 at 12% MC4th lightest of 15540% below the U.S. hardwoods median0.250.96Cupping tendency
2.3910th highest of 15527% above the U.S. hardwoods median1.092.90Bending strength
8,500 psi58.6 MPa13th weakest of 15535% below the U.S. hardwoods median4,300 psi29,900 psiStiffness
1.27 M psi8.8 GPa25th most flexible of 1550.54 M psi4.06 M psiShrinkage across the face
8.6%radial 3.6%52nd highest of 1553.5%12.7%
How much it moves
Most of its movement runs along the rings (T/R 2.39): quartersawn, the same board would lose 0.22 in. instead of 0.52 in.
0.52 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 8.6%
- Radial
- 3.6%
- Volume
- 12.4%
- T/R ratio
- 2.39 (146th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Eastern cottonwood
23% harder · 19% heavier · shrinks 0.6 points more across the face
- Cuangare
9% harder · same density · shrinks 0.8 points more across the face
- Light red meranti
31% harder · 10% heavier · shrinks 0.1 points less across the face
Among the aspens and cottonwoods
2nd hardest of 3, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: the lowest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 160psi | 300psi | +88% | 2.10MPa |
| Side hardness | 250lbf | 350lbf | +40% | 1,557N |
| Compression parallel to grain | 2,200psi | 4,500psi | +105% | 31MPa |
| Modulus of rupture | 4,900psi | 8,500psi | +73% | 58.6MPa |
| Work to maximum load | 5.00in-lbf/in³ | 6.70in-lbf/in³ | +34% | 46.2kJ/m³ |
| Shear parallel to grain | 610psi | 1,040psi | +70% | 7.20MPa |
| Modulus of elasticity | 1.08M psi | 1.27M psi | +18% | 8.76GPa |
| Tension perpendicular | 270psi | 330psi | +22% | 2.30MPa |
| Impact bending | 20in. | 22in. | +10% | 559mm |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides