Peroba rosa
Aspidosperma spp. (peroba group)
Peroba rosa measures 1,730 lbf on the Janka scale, 34% harder than northern red oak.
- It pairs hardness with little movement: harder than 83% of the woods, yet in the lowest quarter for shrinkage across the face.
- Across all 155 woods it falls in the top fifth for hardness and density and in the bottom fifth for face shrinkage.
- On the Janka scale its nearest neighbours are piquia at 1,720 lbf and angelin at 1,750 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Peroba rosaImported woods medianOther woods
Density
0.6625th heaviest of 1550.250.96Janka hardness
1,730 lbf7,695 N27th hardest of 15523rd of 65 imported woods; 33% above the imported woods median240 lbf3,680 lbfShrinkage across the face
6.4%radial 3.8%29th lowest of 1553.5%12.7%Cupping tendency
1.6856th lowest of 1551.092.90Stiffness
1.53 M psi10.6 GPa59th most flexible of 1550.54 M psi4.06 M psiBending strength
12,100 psi83.4 MPa63rd weakest of 15528% below the imported woods median4,300 psi29,900 psi
For its weight: stiffness-to-weight 2.32 (153rd of 155); strength-to-weight 18,333 psi (153rd of 155).
How much it moves
Its face shrinkage of 6.4% is in the lowest quarter of the list, with an ordinary T/R ratio of 1.68.
0.38 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.23 in.
- Tangential
- 6.4%
- Radial
- 3.8%
- Volume
- 11.6%
- T/R ratio
- 1.68 (56th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Honeylocust
9% softer · 9% lighter · shrinks 0.2 points more across the face
- Peroba de campos
8% softer · 6% lighter · shrinks 0.2 points more across the face
- Green ash
31% softer · 20% lighter · shrinks 0.7 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is shear strength: 6th highest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Shear parallel to grain | 1,880psi | 2,490psi | +32% | 17.2MPa |
| Side hardness | 1,580lbf | 1,730lbf | +9% | 7,695N |
| Compression parallel to grain | 5,540psi | 7,920psi | +43% | 54.6MPa |
| Work to maximum load | 10.5in-lbf/in³ | 9.20in-lbf/in³ | −12% | 63.4kJ/m³ |
| Modulus of elasticity | 1.29M psi | 1.53M psi | +19% | 10.6GPa |
| Modulus of rupture | 10,900psi | 12,100psi | +11% | 83.4MPa |