Pignut hickory
Carya glabra
Pignut hickory measures 2,140 lbf on the Janka scale, 66% harder than northern red oak.
- No other U.S. hardwood in the tables is harder or stiffer.
- Among the 53 U.S. hardwoods, only shagbark hickory is stronger in bending.
- Only seven of the 155 woods shrink more across the face.
- Of the four hickories in the handbook, none is heavier.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Pignut hickoryU.S. hardwoods medianOther woods
Shrinkage across the face
11.5%radial 7.2%8th highest of 15529% above the U.S. hardwoods median3.5%12.7%Janka hardness
2,140 lbf9,519 N16th hardest of 1551st of 53 U.S. hardwoods; 84% above the U.S. hardwoods median240 lbf3,680 lbfBending strength
20,100 psi138.6 MPa17th strongest of 15555% above the U.S. hardwoods median4,300 psi29,900 psiStiffness
2.26 M psi15.6 GPa22nd stiffest of 15541% above the U.S. hardwoods median0.54 M psi4.06 M psiDensity
0.660.75 at 12% MC25th heaviest of 15527% above the U.S. hardwoods median0.250.96Cupping tendency
1.6043rd lowest of 1551.092.90
For its weight: strength-to-weight 30,455 psi (13th of 155).
How much it moves
Its face shrinkage of 11.5% is in the top quarter of the list, with an ordinary T/R ratio of 1.60.
0.69 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.43 in.
- Tangential
- 11.5%
- Radial
- 7.2%
- Volume
- 17.9%
- T/R ratio
- 1.60 (43rd most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Mockernut hickory
8% softer · 3% lighter · shrinks 0.5 points less across the face
- Shagbark hickory
12% softer · 3% lighter · shrinks 1.0 points less across the face
- Shellbark hickory
15% softer · 6% lighter · shrinks 1.1 points more across the face
Among the hickories
1st hardest of 4, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: the highest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 920psi | 1,980psi | +115% | 13.7MPa |
| Work to maximum load | 31.7in-lbf/in³ | 30.4in-lbf/in³ | −4% | 209.6kJ/m³ |
| Impact bending | 89in. | 74in. | −17% | 1,880mm |
| Side hardness | 1,520lbf | 2,140lbf | +41% | 9,519N |
| Modulus of rupture | 11,700psi | 20,100psi | +72% | 138.6MPa |
| Shear parallel to grain | 1,370psi | 2,150psi | +57% | 14.8MPa |
| Modulus of elasticity | 1.65M psi | 2.26M psi | +37% | 15.6GPa |
| Compression parallel to grain | 4,810psi | 9,190psi | +91% | 63.4MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides