White fir measures 480 lbf on the Janka scale, about 37% as hard as northern red oak.
- Lodgepole pine and redwood (old-growth) have exactly the same Janka figure.
- Across all 155 woods it falls in the bottom fifth for hardness, density, radial shrinkage and volumetric shrinkage.
- On the Janka scale its nearest neighbours are incense-cedar at 470 lbf and butternut at 490 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
White firU.S. softwoods medianOther woods
Density
0.370.39 at 12% MC23rd lightest of 1550.250.96Janka hardness
480 lbf2,135 N24th softest of 15521st of 37 U.S. softwoods240 lbf3,680 lbfCupping tendency
2.1233rd highest of 1551.092.90Bending strength
9,800 psi67.6 MPa34th weakest of 1554,300 psi29,900 psiShrinkage across the face
7.0%radial 3.3%45th lowest of 1553.5%12.7%Stiffness
1.50 M psi10.3 GPa52nd most flexible of 1550.54 M psi4.06 M psi
How much it moves
Most of its movement runs along the rings (T/R 2.12): quartersawn, the same board would lose 0.20 in. instead of 0.42 in.
0.42 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 7.0%
- Radial
- 3.3%
- Volume
- 9.8%
- T/R ratio
- 2.12 (123rd most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Grand fir
2% harder · 5% lighter · shrinks 0.5 points more across the face
- Jack pine
19% harder · 8% heavier · shrinks 0.4 points less across the face
- Balsam fir
21% softer · 11% lighter · shrinks 0.1 points less across the face
Among the true firs
3rd hardest of 7, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Impact bending | 22in. | 20in. | −9% | 508mm |
| Side hardness | 340lbf | 480lbf | +41% | 2,135N |
| Tension perpendicular | 300psi | 300psi | ±0% | 2.10MPa |
| Work to maximum load | 5.60in-lbf/in³ | 7.20in-lbf/in³ | +29% | 49.6kJ/m³ |
| Shear parallel to grain | 760psi | 1,100psi | +45% | 7.60MPa |
| Modulus of rupture | 5,900psi | 9,800psi | +66% | 67.6MPa |
| Compression perpendicular | 280psi | 530psi | +89% | 3.70MPa |
| Compression parallel to grain | 2,900psi | 5,800psi | +100% | 40MPa |
| Modulus of elasticity | 1.16M psi | 1.50M psi | +29% | 10.3GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides