Mahogany
Swietenia macrophylla
Mahogany measures 800 lbf on the Janka scale, 38% softer than northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
MahoganyImported woods medianOther woods
Shrinkage across the face
4.1%radial 3.0%3rd lowest of 15548% below the imported woods median3.5%12.7%Cupping tendency
1.3710th lowest of 1551.092.90Stiffness
1.50 M psi10.3 GPa52nd most flexible of 15525% below the imported woods median0.54 M psi4.06 M psiDensity
0.4553rd lightest of 15526% below the imported woods median0.250.96Bending strength
11,500 psi79.3 MPa58th weakest of 15531% below the imported woods median4,300 psi29,900 psiJanka hardness
800 lbf3,559 N63rd softest of 15549th of 65 imported woods; 38% below the imported woods median240 lbf3,680 lbf
How much it moves
Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.
0.25 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.18 in.
- Tangential
- 4.1%
- Radial
- 3.0%
- Volume
- 7.8%
- T/R ratio
- 1.37 (10th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- African mahogany
4% harder · 7% lighter · shrinks 0.4 points more across the face
- Iroko
58% harder · 20% heavier · shrinks 0.3 points less across the face
- Albarco
28% harder · 7% heavier · shrinks 1.3 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 9.10in-lbf/in³ | 7.50in-lbf/in³ | −18% | 51.7kJ/m³ |
| Shear parallel to grain | 1,240psi | 1,230psi | −1% | 8.50MPa |
| Modulus of elasticity | 1.34M psi | 1.50M psi | +12% | 10.3GPa |
| Modulus of rupture | 9,000psi | 11,500psi | +28% | 79.3MPa |
| Side hardness | 740lbf | 800lbf | +8% | 3,559N |
| Compression parallel to grain | 4,340psi | 6,780psi | +56% | 46.7MPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides