American sycamore
Platanus occidentalis
American sycamore measures 770 lbf on the Janka scale, 40% softer than northern red oak.
- Yellow meranti has exactly the same Janka figure.
- On the Janka scale its nearest neighbours are Virginia pine at 740 lbf and dark red meranti at 780 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
American sycamoreU.S. hardwoods medianOther woods
Bending strength
10,000 psi68.9 MPa38th weakest of 1554,300 psi29,900 psiStiffness
1.42 M psi9.8 GPa39th most flexible of 1550.54 M psi4.06 M psiCupping tendency
1.6856th lowest of 1551.092.90Density
0.460.49 at 12% MC58th lightest of 1550.250.96Janka hardness
770 lbf3,425 N59th softest of 15543rd of 53 U.S. hardwoods; 34% below the U.S. hardwoods median240 lbf3,680 lbfShrinkage across the face
8.4%radial 5.0%59th highest of 1553.5%12.7%
For its weight: strength-to-weight 21,739 psi (144th of 155).
How much it moves
Both its face shrinkage (8.4%) and its T/R ratio (1.68) sit in the middle half of the list.
0.50 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.30 in.
- Tangential
- 8.4%
- Radial
- 5.0%
- Volume
- 14.1%
- T/R ratio
- 1.68 (56th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Black tupelo
5% harder · same density · shrinks 0.3 points more across the face
- Hackberry
14% harder · 6% heavier · shrinks 0.5 points more across the face
- Ilomba
21% softer · 13% lighter · same face shrinkage
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression parallel to grain | 2,920psi | 5,380psi | +84% | 37.1MPa |
| Tension perpendicular | 630psi | 720psi | +14% | 5.00MPa |
| Modulus of rupture | 6,500psi | 10,000psi | +54% | 68.9MPa |
| Modulus of elasticity | 1.06M psi | 1.42M psi | +34% | 9.79GPa |
| Work to maximum load | 7.50in-lbf/in³ | 8.50in-lbf/in³ | +13% | 58.6kJ/m³ |
| Impact bending | 26in. | 26in. | ±0% | 660mm |
| Side hardness | 610lbf | 770lbf | +26% | 3,425N |
| Compression perpendicular | 360psi | 700psi | +94% | 4.80MPa |
| Shear parallel to grain | 1,000psi | 1,470psi | +47% | 10.1MPa |