Cuangare
Dialyanthera spp.
Cuangare measures 380 lbf on the Janka scale, about 29% as hard as northern red oak.
- No other wood in the tables is stiffer for its weight.
- Only ceiba, northern white-cedar and obeche are lighter, only ceiba, northern white-cedar and Atlantic white-cedar are weaker in bending, and only seven woods are softer.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
CuangareImported woods medianOther woods
Density
0.314th lightest of 15549% below the imported woods median0.250.96Bending strength
7,300 psi50.3 MPa4th weakest of 15556% below the imported woods median4,300 psi29,900 psiJanka hardness
380 lbf1,690 N8th softest of 15563rd of 65 imported woods; 71% below the imported woods median240 lbf3,680 lbfCupping tendency
2.2418th highest of 15529% above the imported woods median1.092.90Shrinkage across the face
9.4%radial 4.2%35th highest of 1553.5%12.7%Stiffness
1.52 M psi10.5 GPa57th most flexible of 1550.54 M psi4.06 M psi
For its weight: stiffness-to-weight 4.90 (1st of 155).
How much it moves
Most of its movement runs along the rings (T/R 2.24): quartersawn, the same board would lose 0.25 in. instead of 0.56 in.
0.56 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 9.4%
- Radial
- 4.2%
- Volume
- 12.0%
- T/R ratio
- 2.24 (138th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Eastern cottonwood
13% harder · 19% heavier · shrinks 0.2 points less across the face
- Black cottonwood
8% softer · same density · shrinks 0.8 points less across the face
- Light red meranti
21% harder · 10% heavier · shrinks 0.9 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is shear strength: 3rd lowest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Shear parallel to grain | 590psi | 830psi | +41% | 5.70MPa |
| Modulus of rupture | 4,000psi | 7,300psi | +82% | 50.3MPa |
| Side hardness | 230lbf | 380lbf | +65% | 1,690N |
| Compression parallel to grain | 2,080psi | 4,760psi | +129% | 32.8MPa |
| Modulus of elasticity | 1.01M psi | 1.52M psi | +50% | 10.5GPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides