TimberLedger

Incense-cedar

Calocedrus decurrens

U.S. softwood · United States

Incense-cedar measures 470 lbf on the Janka scale, about 36% as hard as northern red oak.

  • Of the 155 woods, only six bend more easily, seven lose less volume on drying and eight are weaker in bending.
  • It is soft and steady at once, in the lowest quarter of the list for both hardness and shrinkage across the face.

Compare incense-cedar

U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak

Incense-cedar · 470 lbfCeibaBlack cherryNorthern red oakShagbark hickoryIpe01,0002,0003,0004,000 lbf← softerharder →Ceiba, 240 lbfNorthern white-cedar, 320 lbfAtlantic white-cedar, 350 lbfBlack cottonwood, 350 lbfQuaking aspen, 350 lbfSubalpine fir, 350 lbfWestern redcedar, 350 lbfBalsam fir, 380 lbfCuangare, 380 lbfEastern white pine, 380 lbfOkoume, 380 lbfSugar pine, 380 lbfEngelmann spruce, 390 lbfAmerican basswood, 410 lbfNoble fir, 410 lbfRedwood (young-growth), 420 lbfWestern white pine, 420 lbfEastern cottonwood, 430 lbfObeche, 430 lbfPacific silver fir, 430 lbfLight red meranti, 460 lbfPonderosa pine, 460 lbfLodgepole pine, 480 lbfRedwood (old-growth), 480 lbfWhite fir, 480 lbfButternut, 490 lbfGrand fir, 490 lbfLimba, 490 lbfCalifornia red fir, 500 lbfEastern hemlock, 500 lbfBanak, 510 lbfSitka spruce, 510 lbfBlack spruce, 530 lbfAmerican chestnut, 540 lbfWestern hemlock, 540 lbfYellow-poplar, 540 lbfHura, 550 lbfRed pine, 560 lbfJack pine, 570 lbfYellow-cedar, 580 lbfRed alder, 590 lbfTamarack, 590 lbfDouglas-fir (Interior North), 600 lbfSpanish-cedar, 600 lbfIlomba, 610 lbfCativo, 630 lbfPort-Orford-cedar, 630 lbfDeterma, 660 lbfDouglas-fir (Interior West), 660 lbfPrimavera, 660 lbfMountain hemlock, 680 lbfLoblolly pine, 690 lbfShortleaf pine, 690 lbfCucumbertree, 700 lbfSilver maple, 700 lbfDouglas-fir (Coast), 710 lbfVirginia pine, 740 lbfAmerican sycamore, 770 lbfYellow meranti, 770 lbfDark red meranti, 780 lbfParana-pine, 780 lbfMahogany, 800 lbfBlack tupelo, 810 lbfAfrican mahogany, 830 lbfAmerican elm, 830 lbfWestern larch, 830 lbfBigleaf maple, 850 lbfBlack ash, 850 lbfSweetgum, 850 lbfSlippery elm, 860 lbfLongleaf pine, 870 lbfHackberry, 880 lbfWater tupelo, 880 lbfSande, 900 lbfOcote pine, 910 lbfPaper birch, 910 lbfBlack cherry, 950 lbfRed maple, 950 lbfRoble, 960 lbfTeak, 1,000 lbfBlack walnut, 1,010 lbfAlbarco, 1,020 lbfSouthern magnolia, 1,020 lbfSouthern red oak, 1,060 lbfAvodire, 1,080 lbfManni, 1,120 lbfAndiroba, 1,130 lbfChestnut oak, 1,130 lbfOregon ash, 1,160 lbfBlack maple, 1,180 lbfOvercup oak, 1,190 lbfWater oak, 1,190 lbfGreen ash, 1,200 lbfBlack oak, 1,210 lbfLaurel oak, 1,210 lbfKapur, 1,230 lbfCaribbean pine, 1,240 lbfSwamp chestnut oak, 1,240 lbfIroko, 1,260 lbfYellow birch, 1,260 lbfKeruing, 1,270 lbfAngelique, 1,290 lbfMersawa, 1,290 lbfNorthern red oak, 1,290 lbfAmerican beech, 1,300 lbfRamin, 1,300 lbfRock elm, 1,320 lbfWhite ash, 1,320 lbfPost oak, 1,360 lbfWhite oak, 1,360 lbfBur oak, 1,370 lbfScarlet oak, 1,400 lbfSepetir, 1,410 lbfSugar maple, 1,450 lbfWillow oak, 1,460 lbfSweet birch, 1,470 lbfPin oak, 1,510 lbfSapele, 1,510 lbfAfrormosia, 1,560 lbfHoneylocust, 1,580 lbfPeroba de campos, 1,600 lbfOpepe, 1,630 lbfBlack locust, 1,700 lbfPilon, 1,700 lbfKempas, 1,710 lbfPara-angelim, 1,720 lbfPiquia, 1,720 lbfPeroba rosa, 1,730 lbfAngelin, 1,750 lbfBenge, 1,750 lbfShellbark hickory, 1,810 lbfPurpleheart, 1,860 lbfShagbark hickory, 1,880 lbfJarrah, 1,910 lbfDegame, 1,940 lbfMockernut hickory, 1,970 lbfKarri, 2,040 lbfPignut hickory, 2,140 lbfSucupira, 2,140 lbfGoncalo alves, 2,160 lbfMora, 2,300 lbfCourbaril, 2,350 lbfGreenheart, 2,350 lbfTropical oak (roble), 2,500 lbfBubinga, 2,690 lbfBrazilian rosewood, 2,720 lbfKaneelhart, 2,900 lbfMacawood, 3,150 lbfIndian rosewood, 3,170 lbfBulletwood, 3,190 lbfAzobe, 3,350 lbfManbarklak, 3,480 lbfMarishballi, 3,570 lbfIpe, 3,680 lbfIncense-cedar · 470 lbfNorthern red oakIpe01,0002,0003,0004,000 lbf← softerharder →

Six measures

Incense-cedarU.S. softwoods medianOther woods

  • Stiffness

    1.04 M psi7.2 GPa7th most flexible of 155
    0.54 M psi4.06 M psi
    31% below the U.S. softwoods median
  • Bending strength

    8,000 psi55.2 MPa9th weakest of 155
    4,300 psi29,900 psi
  • Shrinkage across the face

    5.2%radial 3.3%13th lowest of 155
    3.5%12.7%
    27% below the U.S. softwoods median
  • Density

    0.350.37 at 12% MC17th lightest of 155
    0.250.96
  • Janka hardness

    470 lbf2,091 N23rd softest of 155
    240 lbf3,680 lbf
    24th of 37 U.S. softwoods
  • Cupping tendency

    1.5837th lowest of 155
    1.092.90

How much it moves

Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.

0.31 in.

off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.20 in.

Tangential
5.2%
Radial
3.3%
Volume
7.7%
T/R ratio
1.58 (37th most stable of 155)
6 in. green (dashed)5.69 in. dry · −5.2%
Flatsawn
6 in. green (dashed)5.80 in. dry · −3.3%
Quartersawn

End view, shrinkage drawn 3× life size.

Closest substitutes

Compare with the first two

Woods of similar hardness

The eight nearest on the Janka scale, lbf.

Laboratory values

Its most unusual laboratory figure is shear strength: 6th lowest of the 154 woods with a published value.

PropertyGreenDry, 12% MCChange when driedMetric, 12% MC
Shear parallel to grain830psi880psi+6%6.10MPa
Work to maximum load6.40in-lbf/in³5.40in-lbf/in³−16%37.2kJ/m³
Modulus of elasticity0.84M psi1.04M psi+24%7.17GPa
Impact bending17in.17in.±0%432mm
Modulus of rupture6,200psi8,000psi+29%55.2MPa
Tension perpendicular280psi270psi−4%1.90MPa
Compression parallel to grain3,150psi5,200psi+65%35.9MPa
Side hardness390lbf470lbf+21%2,091N
Compression perpendicular370psi590psi+59%4.10MPa

Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides