Redwood (young-growth) measures 420 lbf on the Janka scale, about 33% as hard as northern red oak.

Compare redwood (young-growth)

U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak

Redwood (young-growth) · 420 lbfBlack cherryNorthern red oakShagbark hickoryIpe01,0002,0003,0004,000 lbf← softerharder →Ceiba, 240 lbfNorthern white-cedar, 320 lbfAtlantic white-cedar, 350 lbfBlack cottonwood, 350 lbfQuaking aspen, 350 lbfSubalpine fir, 350 lbfWestern redcedar, 350 lbfBalsam fir, 380 lbfCuangare, 380 lbfEastern white pine, 380 lbfOkoume, 380 lbfSugar pine, 380 lbfEngelmann spruce, 390 lbfAmerican basswood, 410 lbfNoble fir, 410 lbfWestern white pine, 420 lbfEastern cottonwood, 430 lbfObeche, 430 lbfPacific silver fir, 430 lbfLight red meranti, 460 lbfPonderosa pine, 460 lbfIncense-cedar, 470 lbfLodgepole pine, 480 lbfRedwood (old-growth), 480 lbfWhite fir, 480 lbfButternut, 490 lbfGrand fir, 490 lbfLimba, 490 lbfCalifornia red fir, 500 lbfEastern hemlock, 500 lbfBanak, 510 lbfSitka spruce, 510 lbfBlack spruce, 530 lbfAmerican chestnut, 540 lbfWestern hemlock, 540 lbfYellow-poplar, 540 lbfHura, 550 lbfRed pine, 560 lbfJack pine, 570 lbfYellow-cedar, 580 lbfRed alder, 590 lbfTamarack, 590 lbfDouglas-fir (Interior North), 600 lbfSpanish-cedar, 600 lbfIlomba, 610 lbfCativo, 630 lbfPort-Orford-cedar, 630 lbfDeterma, 660 lbfDouglas-fir (Interior West), 660 lbfPrimavera, 660 lbfMountain hemlock, 680 lbfLoblolly pine, 690 lbfShortleaf pine, 690 lbfCucumbertree, 700 lbfSilver maple, 700 lbfDouglas-fir (Coast), 710 lbfVirginia pine, 740 lbfAmerican sycamore, 770 lbfYellow meranti, 770 lbfDark red meranti, 780 lbfParana-pine, 780 lbfMahogany, 800 lbfBlack tupelo, 810 lbfAfrican mahogany, 830 lbfAmerican elm, 830 lbfWestern larch, 830 lbfBigleaf maple, 850 lbfBlack ash, 850 lbfSweetgum, 850 lbfSlippery elm, 860 lbfLongleaf pine, 870 lbfHackberry, 880 lbfWater tupelo, 880 lbfSande, 900 lbfOcote pine, 910 lbfPaper birch, 910 lbfBlack cherry, 950 lbfRed maple, 950 lbfRoble, 960 lbfTeak, 1,000 lbfBlack walnut, 1,010 lbfAlbarco, 1,020 lbfSouthern magnolia, 1,020 lbfSouthern red oak, 1,060 lbfAvodire, 1,080 lbfManni, 1,120 lbfAndiroba, 1,130 lbfChestnut oak, 1,130 lbfOregon ash, 1,160 lbfBlack maple, 1,180 lbfOvercup oak, 1,190 lbfWater oak, 1,190 lbfGreen ash, 1,200 lbfBlack oak, 1,210 lbfLaurel oak, 1,210 lbfKapur, 1,230 lbfCaribbean pine, 1,240 lbfSwamp chestnut oak, 1,240 lbfIroko, 1,260 lbfYellow birch, 1,260 lbfKeruing, 1,270 lbfAngelique, 1,290 lbfMersawa, 1,290 lbfNorthern red oak, 1,290 lbfAmerican beech, 1,300 lbfRamin, 1,300 lbfRock elm, 1,320 lbfWhite ash, 1,320 lbfPost oak, 1,360 lbfWhite oak, 1,360 lbfBur oak, 1,370 lbfScarlet oak, 1,400 lbfSepetir, 1,410 lbfSugar maple, 1,450 lbfWillow oak, 1,460 lbfSweet birch, 1,470 lbfPin oak, 1,510 lbfSapele, 1,510 lbfAfrormosia, 1,560 lbfHoneylocust, 1,580 lbfPeroba de campos, 1,600 lbfOpepe, 1,630 lbfBlack locust, 1,700 lbfPilon, 1,700 lbfKempas, 1,710 lbfPara-angelim, 1,720 lbfPiquia, 1,720 lbfPeroba rosa, 1,730 lbfAngelin, 1,750 lbfBenge, 1,750 lbfShellbark hickory, 1,810 lbfPurpleheart, 1,860 lbfShagbark hickory, 1,880 lbfJarrah, 1,910 lbfDegame, 1,940 lbfMockernut hickory, 1,970 lbfKarri, 2,040 lbfPignut hickory, 2,140 lbfSucupira, 2,140 lbfGoncalo alves, 2,160 lbfMora, 2,300 lbfCourbaril, 2,350 lbfGreenheart, 2,350 lbfTropical oak (roble), 2,500 lbfBubinga, 2,690 lbfBrazilian rosewood, 2,720 lbfKaneelhart, 2,900 lbfMacawood, 3,150 lbfIndian rosewood, 3,170 lbfBulletwood, 3,190 lbfAzobe, 3,350 lbfManbarklak, 3,480 lbfMarishballi, 3,570 lbfIpe, 3,680 lbfRedwood (young-growth) · 420 lbfNorthern red oakIpe01,0002,0003,0004,000 lbf← softerharder →

Six measures

Redwood (young-growth)U.S. softwoods medianOther woods

  • Bending strength

    7,900 psi54.5 MPa8th weakest of 155
    4,300 psi29,900 psi
  • Stiffness

    1.10 M psi7.6 GPa9th most flexible of 155
    0.54 M psi4.06 M psi
    27% below the U.S. softwoods median
  • Shrinkage across the face

    4.9%radial 2.2%9th lowest of 155
    3.5%12.7%
    31% below the U.S. softwoods median
  • Density

    0.340.35 at 12% MC13th lightest of 155
    0.250.96
  • Janka hardness

    420 lbf1,868 N16th softest of 155
    240 lbf3,680 lbf
    27th of 37 U.S. softwoods
  • Cupping tendency

    2.2319th highest of 155
    1.092.90

How much it moves

Total movement is small, but most of it runs along the rings (T/R 2.23), so a flatsawn board still loses 2.2 times the width of a quartersawn one.

0.29 in.

off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.13 in.

Tangential
4.9%
Radial
2.2%
Volume
7.0%
T/R ratio
2.23 (135th most stable of 155)
6 in. green (dashed)5.71 in. dry · −4.9%
Flatsawn
6 in. green (dashed)5.87 in. dry · −2.2%
Quartersawn

End view, shrinkage drawn 3× life size.

Closest substitutes

  • Western redcedar

    17% softer · 9% lighter · shrinks 0.1 points more across the face

  • Sugar pine

    10% softer · same density · shrinks 0.7 points more across the face

  • Eastern white pine

    10% softer · same density · shrinks 1.2 points more across the face

Compare with the first two

Woods of similar hardness

The eight nearest on the Janka scale, lbf.

Laboratory values

Its most unusual laboratory figure is impact bending height: 3rd lowest of the 89 woods with a published value.

PropertyGreenDry, 12% MCChange when driedMetric, 12% MC
Impact bending16in.15in.−6%381mm
Work to maximum load5.70in-lbf/in³5.20in-lbf/in³−9%35.9kJ/m³
Modulus of rupture5,900psi7,900psi+34%54.5MPa
Modulus of elasticity0.96M psi1.10M psi+15%7.58GPa
Tension perpendicular300psi250psi−17%1.70MPa
Side hardness350lbf420lbf+20%1,868N
Compression parallel to grain3,110psi5,220psi+68%36MPa
Compression perpendicular270psi520psi+93%3.60MPa
Shear parallel to grain890psi1,110psi+25%7.70MPa

Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides