Oregon ash measures 1,160 lbf on the Janka scale, 10% softer than northern red oak.
- Of the four ashes in the handbook, none bends more easily, shrinks more across the face or has a higher T/R ratio.
- On the Janka scale its nearest neighbours are chestnut oak at 1,130 lbf and black maple at 1,180 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Oregon ashU.S. hardwoods medianOther woods
Stiffness
1.36 M psi9.4 GPa34th most flexible of 1550.54 M psi4.06 M psiCupping tendency
1.9847th highest of 1551.092.90Janka hardness
1,160 lbf5,160 N66th hardest of 15527th of 53 U.S. hardwoods240 lbf3,680 lbfShrinkage across the face
8.1%radial 4.1%66th highest of 1553.5%12.7%Bending strength
12,700 psi87.6 MPa74th weakest of 1554,300 psi29,900 psiDensity
0.500.55 at 12% MC76th heaviest of 1550.250.96
For its weight: stiffness-to-weight 2.72 (139th of 155).
How much it moves
Both its face shrinkage (8.1%) and its T/R ratio (1.98) sit in the middle half of the list.
0.49 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.25 in.
- Tangential
- 8.1%
- Radial
- 4.1%
- Volume
- 13.2%
- T/R ratio
- 1.98 (108th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Red maple
18% softer · 2% lighter · shrinks 0.1 points more across the face
- Black cherry
18% softer · 6% lighter · shrinks 1.0 points less across the face
- Avodire
7% softer · 4% lighter · shrinks 1.4 points less across the face
Among the ashes
3rd hardest of 4, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 530psi | 1,250psi | +136% | 8.60MPa |
| Tension perpendicular | 590psi | 720psi | +22% | 5.00MPa |
| Modulus of elasticity | 1.13M psi | 1.36M psi | +20% | 9.38GPa |
| Work to maximum load | 12.2in-lbf/in³ | 14.4in-lbf/in³ | +18% | 99.3kJ/m³ |
| Compression parallel to grain | 3,510psi | 6,040psi | +72% | 41.6MPa |
| Impact bending | 39in. | 33in. | −15% | 838mm |
| Shear parallel to grain | 1,190psi | 1,790psi | +50% | 12.3MPa |
| Side hardness | 790lbf | 1,160lbf | +47% | 5,160N |
| Modulus of rupture | 7,600psi | 12,700psi | +67% | 87.6MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides