Rock elm
Ulmus thomasii
Rock elm measures 1,320 lbf on the Janka scale, 2% harder than northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Rock elmU.S. hardwoods medianOther woods
Janka hardness
1,320 lbf5,872 N47th hardest of 15515th of 53 U.S. hardwoods240 lbf3,680 lbfDensity
0.570.63 at 12% MC49th heaviest of 1550.250.96Bending strength
14,800 psi102.0 MPa53rd strongest of 1554,300 psi29,900 psiCupping tendency
1.6958th lowest of 1551.092.90Stiffness
1.54 M psi10.6 GPa60th most flexible of 1550.54 M psi4.06 M psiShrinkage across the face
8.1%radial 4.8%66th highest of 1553.5%12.7%
For its weight: stiffness-to-weight 2.70 (142nd of 155).
How much it moves
Both its face shrinkage (8.1%) and its T/R ratio (1.69) sit in the middle half of the list.
0.49 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.29 in.
- Tangential
- 8.1%
- Radial
- 4.8%
- Volume
- 14.9%
- T/R ratio
- 1.69 (58th most stable of 155)
End view, shrinkage drawn 3× life size.
Laboratory values
Its most unusual laboratory figure is impact bending height: 6th highest of the 89 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Impact bending | 54in. | 56in. | +4% | 1,422mm |
| Work to maximum load | 19.8in-lbf/in³ | 19.2in-lbf/in³ | −3% | 132.4kJ/m³ |
| Compression perpendicular | 610psi | 1,230psi | +102% | 8.50MPa |
| Shear parallel to grain | 1,270psi | 1,920psi | +51% | 13.2MPa |
| Side hardness | 940lbf | 1,320lbf | +40% | 5,872N |
| Modulus of rupture | 9,500psi | 14,800psi | +56% | 102MPa |
| Modulus of elasticity | 1.19M psi | 1.54M psi | +29% | 10.6GPa |
| Compression parallel to grain | 3,780psi | 7,050psi | +87% | 48.6MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides