Avodire
Turraeanthus africanus
Avodire measures 1,080 lbf on the Janka scale, 16% softer than northern red oak.
- Across all 155 woods it falls in the bottom fifth for T/R ratio.
- On the Janka scale its nearest neighbours are southern red oak at 1,060 lbf and manni at 1,120 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
AvodireImported woods medianOther woods
Cupping tendency
1.4620th lowest of 1551.092.90Shrinkage across the face
6.7%radial 4.6%36th lowest of 1553.5%12.7%Stiffness
1.49 M psi10.3 GPa48th most flexible of 15526% below the imported woods median0.54 M psi4.06 M psiJanka hardness
1,080 lbf4,804 N70th hardest of 15542nd of 65 imported woods240 lbf3,680 lbfDensity
0.4871st lightest of 1550.250.96Bending strength
12,700 psi87.6 MPa74th weakest of 1554,300 psi29,900 psi
How much it moves
Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.
0.40 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.28 in.
- Tangential
- 6.7%
- Radial
- 4.6%
- Volume
- 12.0%
- T/R ratio
- 1.46 (20th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Green ash
11% harder · 10% heavier · shrinks 0.4 points more across the face
- Southern magnolia
6% softer · 4% lighter · shrinks 0.1 points less across the face
- Black cherry
12% softer · 2% lighter · shrinks 0.4 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Dry, 12% MC | Metric, 12% MC |
|---|---|---|
| Shear parallel to grain | 2,030psi | 14MPa |
| Modulus of elasticity | 1.49M psi | 10.3GPa |
| Work to maximum load | 9.40in-lbf/in³ | 64.8kJ/m³ |
| Compression parallel to grain | 7,150psi | 49.3MPa |
| Side hardness | 1,080lbf | 4,804N |
| Modulus of rupture | 12,700psi | 87.6MPa |
The handbook publishes only values at 12% moisture content for this wood; green values and some tests are not given.
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides