Macawood measures 3,150 lbf on the Janka scale, 144% harder than northern red oak.
- No other wood in the tables shrinks less across the face or loses less volume on drying.
- Only kaneelhart is heavier, and only kaneelhart and marishballi are stronger in bending.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
MacawoodImported woods medianOther woods
Shrinkage across the face
3.5%radial 2.7%1st lowest of 15556% below the imported woods median3.5%12.7%Density
0.942nd heaviest of 15554% above the imported woods median0.250.96Bending strength
27,600 psi190.3 MPa3rd strongest of 15565% above the imported woods median4,300 psi29,900 psiStiffness
3.20 M psi22.1 GPa5th stiffest of 15560% above the imported woods median0.54 M psi4.06 M psiCupping tendency
1.306th lowest of 15525% below the imported woods median1.092.90Janka hardness
3,150 lbf14,012 N7th hardest of 1557th of 65 imported woods; 142% above the imported woods median240 lbf3,680 lbf
For its weight: strength-to-weight 29,362 psi (20th of 155).
How much it moves
Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.
0.21 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.16 in.
- Tangential
- 3.5%
- Radial
- 2.7%
- Volume
- 6.5%
- T/R ratio
- 1.30 (6th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Sucupira
32% softer · 17% lighter · shrinks 3.5 points more across the face
- Brazilian rosewood
14% softer · 15% lighter · shrinks 1.1 points more across the face
- Purpleheart
41% softer · 29% lighter · shrinks 2.6 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength along the grain: 2nd highest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression parallel to grain | 10,540psi | 16,100psi | +53% | 111MPa |
| Modulus of rupture | 22,300psi | 27,600psi | +24% | 190.3MPa |
| Shear parallel to grain | 1,840psi | 2,540psi | +38% | 17.5MPa |
| Modulus of elasticity | 3.02M psi | 3.20M psi | +6% | 22.1GPa |
| Side hardness | 3,320lbf | 3,150lbf | −5% | 14,012N |
Note on the data: the published side hardness at 12% MC is lower than the green value.