Eastern cottonwood
Populus deltoides
Eastern cottonwood measures 430 lbf on the Janka scale, about 33% as hard as northern red oak.
- Of the three aspens and cottonwoods in the handbook, none is harder, heavier or stiffer, and none shrinks more across the face.
- Obeche and Pacific silver fir have exactly the same Janka figure.
- Across all 155 woods it falls in the top fifth for T/R ratio and in the bottom fifth for hardness, density and bending strength.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Eastern cottonwoodU.S. hardwoods medianOther woods
Cupping tendency
2.3612th highest of 15526% above the U.S. hardwoods median1.092.90Bending strength
8,500 psi58.6 MPa13th weakest of 15535% below the U.S. hardwoods median4,300 psi29,900 psiJanka hardness
430 lbf1,913 N18th softest of 15550th of 53 U.S. hardwoods; 63% below the U.S. hardwoods median240 lbf3,680 lbfDensity
0.370.40 at 12% MC23rd lightest of 15529% below the U.S. hardwoods median0.250.96Stiffness
1.37 M psi9.4 GPa35th most flexible of 1550.54 M psi4.06 M psiShrinkage across the face
9.2%radial 3.9%39th highest of 1553.5%12.7%
How much it moves
Most of its movement runs along the rings (T/R 2.36): quartersawn, the same board would lose 0.23 in. instead of 0.55 in.
0.55 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 9.2%
- Radial
- 3.9%
- Volume
- 13.9%
- T/R ratio
- 2.36 (144th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Cuangare
12% softer · 16% lighter · shrinks 0.2 points more across the face
- Black cottonwood
19% softer · 16% lighter · shrinks 0.6 points less across the face
- Light red meranti
7% harder · 8% lighter · shrinks 0.7 points less across the face
Among the aspens and cottonwoods
1st hardest of 3, lbf.
Laboratory values
Its most unusual laboratory figure is crushing strength across the grain: 5th lowest of the 90 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Compression perpendicular | 200psi | 380psi | +90% | 2.60MPa |
| Shear parallel to grain | 680psi | 930psi | +37% | 6.40MPa |
| Modulus of rupture | 5,300psi | 8,500psi | +60% | 58.6MPa |
| Side hardness | 340lbf | 430lbf | +26% | 1,913N |
| Compression parallel to grain | 2,280psi | 4,910psi | +115% | 33.9MPa |
| Impact bending | 21in. | 20in. | −5% | 508mm |
| Work to maximum load | 7.30in-lbf/in³ | 7.40in-lbf/in³ | +1% | 51kJ/m³ |
| Modulus of elasticity | 1.01M psi | 1.37M psi | +36% | 9.45GPa |
| Tension perpendicular | 410psi | 580psi | +41% | 4.00MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides