Lodgepole pine measures 480 lbf on the Janka scale, about 37% as hard as northern red oak.
- It is soft and steady at once, in the lowest quarter of the list for both hardness and shrinkage across the face.
- Redwood (old-growth) and white fir have exactly the same Janka figure.
- Across all 155 woods it falls in the bottom fifth for hardness, density, bending strength, stiffness and T/R ratio.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Lodgepole pineU.S. softwoods medianOther woods
Janka hardness
480 lbf2,135 N24th softest of 15521st of 37 U.S. softwoods240 lbf3,680 lbfBending strength
9,400 psi64.8 MPa27th weakest of 1554,300 psi29,900 psiDensity
0.380.41 at 12% MC28th lightest of 1550.250.96Stiffness
1.34 M psi9.2 GPa30th most flexible of 1550.54 M psi4.06 M psiCupping tendency
1.5631st lowest of 1551.092.90Shrinkage across the face
6.7%radial 4.3%36th lowest of 1553.5%12.7%
How much it moves
Little movement, and evenly split between the two directions: one of the steadiest woods in the tables.
0.40 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.26 in.
- Tangential
- 6.7%
- Radial
- 4.3%
- Volume
- 11.1%
- T/R ratio
- 1.56 (31st most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Ponderosa pine
4% softer · same density · shrinks 0.5 points less across the face
- Western white pine
12% softer · 8% lighter · shrinks 0.7 points more across the face
- Jack pine
19% harder · 5% heavier · shrinks 0.1 points less across the face
Among the pines
9th hardest of 13, lbf; the neighbours either side are shown, the rest are on the pines page.
Laboratory values
Its most unusual laboratory figure is shear strength: 6th lowest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Shear parallel to grain | 680psi | 880psi | +29% | 6.10MPa |
| Work to maximum load | 5.60in-lbf/in³ | 6.80in-lbf/in³ | +21% | 46.9kJ/m³ |
| Impact bending | 20in. | 20in. | ±0% | 508mm |
| Tension perpendicular | 220psi | 290psi | +32% | 2.00MPa |
| Side hardness | 330lbf | 480lbf | +45% | 2,135N |
| Modulus of rupture | 5,500psi | 9,400psi | +71% | 64.8MPa |
| Compression parallel to grain | 2,610psi | 5,370psi | +106% | 37MPa |
| Modulus of elasticity | 1.08M psi | 1.34M psi | +24% | 9.24GPa |
| Compression perpendicular | 250psi | 610psi | +144% | 4.20MPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides