Quaking aspen
Populus tremuloides
Quaking aspen measures 350 lbf on the Janka scale, about 27% as hard as northern red oak.
- Only ceiba and northern white-cedar are softer.
- Among the 53 U.S. hardwoods, only butternut is weaker in bending.
- Of the three aspens and cottonwoods in the handbook, none bends more easily, shrinks less across the face or has a T/R ratio closer to 1.
- It is soft and steady at once, in the lowest quarter of the list for both hardness and shrinkage across the face.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Quaking aspenU.S. hardwoods medianOther woods
Janka hardness
350 lbf1,557 N3rd softest of 15552nd of 53 U.S. hardwoods; 70% below the U.S. hardwoods median240 lbf3,680 lbfBending strength
8,400 psi57.9 MPa12th weakest of 15535% below the U.S. hardwoods median4,300 psi29,900 psiStiffness
1.18 M psi8.1 GPa15th most flexible of 15526% below the U.S. hardwoods median0.54 M psi4.06 M psiDensity
0.350.38 at 12% MC17th lightest of 15533% below the U.S. hardwoods median0.250.96Shrinkage across the face
6.7%radial 3.5%36th lowest of 1553.5%12.7%Cupping tendency
1.9159th highest of 1551.092.90
How much it moves
Its face shrinkage of 6.7% is in the lowest quarter of the list, with an ordinary T/R ratio of 1.91.
0.40 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.21 in.
- Tangential
- 6.7%
- Radial
- 3.5%
- Volume
- 11.5%
- T/R ratio
- 1.91 (95th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Butternut
40% harder · 3% heavier · shrinks 0.3 points less across the face
- Okoume
9% harder · 6% lighter · shrinks 0.6 points less across the face
- American chestnut
54% harder · 14% heavier · same face shrinkage
Among the aspens and cottonwoods
3rd hardest of 3, lbf.
Laboratory values
Its most unusual laboratory figure is shear strength: 4th lowest of the 154 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Side hardness | 300lbf | 350lbf | +17% | 1,557N |
| Shear parallel to grain | 660psi | 850psi | +29% | 5.90MPa |
| Compression perpendicular | 180psi | 370psi | +106% | 2.60MPa |
| Compression parallel to grain | 2,140psi | 4,250psi | +99% | 29.3MPa |
| Modulus of rupture | 5,100psi | 8,400psi | +65% | 57.9MPa |
| Modulus of elasticity | 0.86M psi | 1.18M psi | +37% | 8.14GPa |
| Tension perpendicular | 230psi | 260psi | +13% | 1.80MPa |
| Impact bending | 22in. | 21in. | −5% | 533mm |
| Work to maximum load | 6.40in-lbf/in³ | 7.60in-lbf/in³ | +19% | 52.4kJ/m³ |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides