Indian rosewood
Dalbergia latifolia
Indian rosewood measures 3,170 lbf on the Janka scale, 146% harder than northern red oak.
- Only five of the 155 woods are harder.
- No wood in the tables sits further above the line linking density and hardness: at a specific gravity of 0.75 the overall trend points to about 2,230 lbf.
- It pairs hardness with little movement: harder than 97% of the woods, yet in the lowest quarter for shrinkage across the face.
- Drying hardens it more than most: from 1,560 lbf green, it gains 103% by 12% moisture, where the median wood gains 31%.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Indian rosewoodImported woods medianOther woods
Janka hardness
3,170 lbf14,101 N6th hardest of 1556th of 65 imported woods; 144% above the imported woods median240 lbf3,680 lbfDensity
0.7515th heaviest of 1550.250.96Shrinkage across the face
5.8%radial 2.7%19th lowest of 15527% below the imported woods median3.5%12.7%Cupping tendency
2.1528th highest of 1551.092.90Bending strength
16,900 psi116.5 MPa37th strongest of 1554,300 psi29,900 psiStiffness
1.78 M psi12.3 GPa61st stiffest of 1550.54 M psi4.06 M psi
For its weight: stiffness-to-weight 2.37 (151st of 155).
How much it moves
Total movement is small, but most of it runs along the rings (T/R 2.15), so a flatsawn board still loses 2.1 times the width of a quartersawn one.
0.35 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.16 in.
- Tangential
- 5.8%
- Radial
- 2.7%
- Volume
- 8.5%
- T/R ratio
- 2.15 (127th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Brazilian rosewood
14% softer · 7% heavier · shrinks 1.2 points less across the face
- Purpleheart
41% softer · 11% lighter · shrinks 0.3 points more across the face
- Afrormosia
51% softer · 19% lighter · shrinks 0.6 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Side hardness | 1,560lbf | 3,170lbf | +103% | 14,101N |
| Shear parallel to grain | 1,400psi | 2,090psi | +49% | 14.4MPa |
| Compression parallel to grain | 4,530psi | 9,220psi | +104% | 63.6MPa |
| Modulus of rupture | 9,200psi | 16,900psi | +84% | 116.5MPa |
| Modulus of elasticity | 1.19M psi | 1.78M psi | +50% | 12.3GPa |
| Work to maximum load | 11.6in-lbf/in³ | 13.1in-lbf/in³ | +13% | 90.3kJ/m³ |