Keruing
Dipterocarpus spp.
Keruing measures 1,270 lbf on the Janka scale, 2% softer than northern red oak.
- No wood in the tables sits further below the line linking density and hardness: at a specific gravity of 0.69 the trend across all 155 woods points to about 1,950 lbf.
- Overall it falls in the top fifth for density, bending strength, face shrinkage and volumetric shrinkage.
- On the Janka scale its nearest neighbours are yellow birch at 1,260 lbf and angelique at 1,290 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
KeruingImported woods medianOther woods
Shrinkage across the face
10.9%radial 5.2%14th highest of 15538% above the imported woods median3.5%12.7%Bending strength
19,900 psi137.2 MPa18th strongest of 1554,300 psi29,900 psiDensity
0.6920th heaviest of 1550.250.96Stiffness
2.07 M psi14.3 GPa33rd stiffest of 1550.54 M psi4.06 M psiCupping tendency
2.1034th highest of 1551.092.90Janka hardness
1,270 lbf5,649 N54th hardest of 15536th of 65 imported woods240 lbf3,680 lbf
How much it moves
Most of its movement runs along the rings (T/R 2.10): quartersawn, the same board would lose 0.31 in. instead of 0.65 in.
0.65 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 10.9%
- Radial
- 5.2%
- Volume
- 16.1%
- T/R ratio
- 2.10 (122nd most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Kapur
3% softer · 7% lighter · shrinks 0.7 points less across the face
- Pilon
34% harder · 6% lighter · shrinks 0.8 points more across the face
- Scarlet oak
10% harder · 13% lighter · shrinks 0.1 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is work to maximum load: 9th highest of the 142 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 13.9in-lbf/in³ | 23.5in-lbf/in³ | +69% | 162kJ/m³ |
| Compression parallel to grain | 5,680psi | 10,500psi | +85% | 72.4MPa |
| Modulus of rupture | 11,900psi | 19,900psi | +67% | 137.2MPa |
| Shear parallel to grain | 1,170psi | 2,070psi | +77% | 14.3MPa |
| Modulus of elasticity | 1.71M psi | 2.07M psi | +21% | 14.3GPa |
| Side hardness | 1,060lbf | 1,270lbf | +20% | 5,649N |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides