Northern white-cedar
Thuja occidentalis
Northern white-cedar measures 320 lbf on the Janka scale, about 25% as hard as northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Northern white-cedarU.S. softwoods medianOther woods
Janka hardness
320 lbf1,423 N2nd softest of 15537th of 37 U.S. softwoods; 36% below the U.S. softwoods median240 lbf3,680 lbfDensity
0.290.31 at 12% MC2nd lightest of 1550.250.96Bending strength
6,500 psi44.8 MPa2nd weakest of 15536% below the U.S. softwoods median4,300 psi29,900 psiStiffness
0.80 M psi5.5 GPa2nd most flexible of 15547% below the U.S. softwoods median0.54 M psi4.06 M psiShrinkage across the face
4.9%radial 2.2%9th lowest of 15531% below the U.S. softwoods median3.5%12.7%Cupping tendency
2.2319th highest of 1551.092.90
For its weight: stiffness-to-weight 2.76 (137th of 155); strength-to-weight 22,414 psi (140th of 155).
How much it moves
Total movement is small, but most of it runs along the rings (T/R 2.23), so a flatsawn board still loses 2.2 times the width of a quartersawn one.
0.29 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.13 in.
- Tangential
- 4.9%
- Radial
- 2.2%
- Volume
- 7.2%
- T/R ratio
- 2.23 (135th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Western redcedar
9% harder · 7% heavier · shrinks 0.1 points more across the face
- Atlantic white-cedar
9% harder · 7% heavier · shrinks 0.5 points more across the face
- Redwood (young-growth)
31% harder · 17% heavier · same face shrinkage
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
Its most unusual laboratory figure is impact bending height: the lowest of the 89 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Impact bending | 15in. | 12in. | −20% | 305mm |
| Modulus of elasticity | 0.64M psi | 0.80M psi | +25% | 5.52GPa |
| Modulus of rupture | 4,200psi | 6,500psi | +55% | 44.8MPa |
| Side hardness | 230lbf | 320lbf | +39% | 1,423N |
| Compression perpendicular | 230psi | 310psi | +35% | 2.10MPa |
| Compression parallel to grain | 1,990psi | 3,960psi | +99% | 27.3MPa |
| Work to maximum load | 5.70in-lbf/in³ | 4.80in-lbf/in³ | −16% | 33.1kJ/m³ |
| Shear parallel to grain | 620psi | 850psi | +37% | 5.90MPa |
| Tension perpendicular | 240psi | 240psi | ±0% | 1.70MPa |