Tamarack
Larix laricina
Tamarack measures 590 lbf on the Janka scale, about 46% as hard as northern red oak.
- Among the 37 U.S. softwoods, only longleaf pine is heavier.
- Only six woods sit further below the density–hardness trend: a specific gravity of 0.49 would point to about 1,010 lbf.
- Red alder has exactly the same Janka figure.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
TamarackU.S. softwoods medianOther woods
Janka hardness
590 lbf2,624 N42nd softest of 15511th of 37 U.S. softwoods240 lbf3,680 lbfCupping tendency
2.0045th highest of 1551.092.90Shrinkage across the face
7.4%radial 3.7%59th lowest of 1553.5%12.7%Bending strength
11,600 psi80.0 MPa61st weakest of 1554,300 psi29,900 psiDensity
0.490.53 at 12% MC76th lightest of 15529% above the U.S. softwoods median0.250.96Stiffness
1.64 M psi11.3 GPa76th stiffest of 1550.54 M psi4.06 M psi
How much it moves
Both its face shrinkage (7.4%) and its T/R ratio (2.00) sit in the middle half of the list.
0.44 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.22 in.
- Tangential
- 7.4%
- Radial
- 3.7%
- Volume
- 13.6%
- T/R ratio
- 2.00 (110th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Douglas-fir (Interior North)
2% harder · 8% lighter · shrinks 0.5 points less across the face
- Red pine
5% softer · 16% lighter · shrinks 0.2 points less across the face
- Western hemlock
8% softer · 14% lighter · shrinks 0.4 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 7.20in-lbf/in³ | 7.10in-lbf/in³ | −1% | 49kJ/m³ |
| Impact bending | 28in. | 23in. | −18% | 584mm |
| Side hardness | 380lbf | 590lbf | +55% | 2,624N |
| Shear parallel to grain | 860psi | 1,280psi | +49% | 8.80MPa |
| Tension perpendicular | 260psi | 400psi | +54% | 2.80MPa |
| Modulus of rupture | 7,200psi | 11,600psi | +61% | 80MPa |
| Compression parallel to grain | 3,480psi | 7,160psi | +106% | 49.4MPa |
| Compression perpendicular | 390psi | 800psi | +105% | 5.50MPa |
| Modulus of elasticity | 1.24M psi | 1.64M psi | +32% | 11.3GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides