Ilomba
Pycnanthus angolensis
Ilomba measures 610 lbf on the Janka scale, about 47% as hard as northern red oak.
- Its bending strength is 41% below the median for imported woods.
- On the Janka scale its nearest neighbours are Spanish-cedar at 600 lbf and cativo at 630 lbf.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
IlombaImported woods medianOther woods
Density
0.4036th lightest of 15534% below the imported woods median0.250.96Bending strength
9,900 psi68.3 MPa36th weakest of 15541% below the imported woods median4,300 psi29,900 psiJanka hardness
610 lbf2,713 N46th softest of 15556th of 65 imported woods; 53% below the imported woods median240 lbf3,680 lbfShrinkage across the face
8.4%radial 4.6%59th highest of 1553.5%12.7%Stiffness
1.59 M psi11.0 GPa66th most flexible of 1550.54 M psi4.06 M psiCupping tendency
1.8374th highest of 1551.092.90
How much it moves
Both its face shrinkage (8.4%) and its T/R ratio (1.83) sit in the middle half of the list.
0.50 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.28 in.
- Tangential
- 8.4%
- Radial
- 4.6%
- Volume
- 12.8%
- T/R ratio
- 1.83 (81st most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Yellow-poplar
12% softer · same density · shrinks 0.2 points less across the face
- American sycamore
26% harder · 15% heavier · same face shrinkage
- Red alder
3% softer · 8% lighter · shrinks 1.1 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Modulus of rupture | 5,500psi | 9,900psi | +80% | 68.3MPa |
| Compression parallel to grain | 2,900psi | 5,550psi | +91% | 38.3MPa |
| Side hardness | 470lbf | 610lbf | +30% | 2,713N |
| Shear parallel to grain | 840psi | 1,290psi | +54% | 8.90MPa |
| Modulus of elasticity | 1.14M psi | 1.59M psi | +39% | 11.0GPa |
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides