White ash
Fraxinus americana
White ash measures 1,320 lbf on the Janka scale, 2% harder than northern red oak.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
White ashU.S. hardwoods medianOther woods
Cupping tendency
1.5939th lowest of 1551.092.90Janka hardness
1,320 lbf5,872 N47th hardest of 15515th of 53 U.S. hardwoods240 lbf3,680 lbfBending strength
15,000 psi103.4 MPa50th strongest of 1554,300 psi29,900 psiDensity
0.550.60 at 12% MC60th heaviest of 1550.250.96Stiffness
1.74 M psi12.0 GPa68th stiffest of 1550.54 M psi4.06 M psiShrinkage across the face
7.8%radial 4.9%76th highest of 1553.5%12.7%
How much it moves
The two directions move almost alike (T/R 1.59), so flatsawn and quartersawn boards differ by only 0.17 in.
0.47 in.
off a 6-inch flatsawn board, green to oven-dry
- Tangential
- 7.8%
- Radial
- 4.9%
- Volume
- 13.3%
- T/R ratio
- 1.59 (39th most stable of 155)
End view, shrinkage drawn 3× life size.
Laboratory values
Its most unusual laboratory figure is tension across the grain: 4th highest of the 73 woods with a published value.
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Tension perpendicular | 590psi | 940psi | +59% | 6.50MPa |
| Compression perpendicular | 670psi | 1,160psi | +73% | 8.00MPa |
| Impact bending | 38in. | 43in. | +13% | 1,092mm |
| Work to maximum load | 15.7in-lbf/in³ | 16.6in-lbf/in³ | +6% | 114.5kJ/m³ |
| Shear parallel to grain | 1,350psi | 1,910psi | +41% | 13.2MPa |
| Side hardness | 960lbf | 1,320lbf | +38% | 5,872N |
| Modulus of rupture | 9,500psi | 15,000psi | +58% | 103.4MPa |
| Compression parallel to grain | 3,990psi | 7,410psi | +86% | 51.1MPa |
| Modulus of elasticity | 1.44M psi | 1.74M psi | +21% | 12GPa |
Wood Handbook Table 5-3b, Table 4-3. Data & method · Guides