Goncalo alves
Astronium graveolens
Goncalo alves measures 2,160 lbf on the Janka scale, 67% harder than northern red oak.
- Only three woods sit further below the density–hardness trend: a specific gravity of 0.84 would point to about 2,650 lbf.
- Only seven of the 155 woods are heavier.
- Overall it falls in the top fifth for hardness and stiffness and in the bottom fifth for volumetric shrinkage.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
Goncalo alvesImported woods medianOther woods
Density
0.848th heaviest of 15538% above the imported woods median0.250.96Janka hardness
2,160 lbf9,608 N15th hardest of 15515th of 65 imported woods; 66% above the imported woods median240 lbf3,680 lbfStiffness
2.23 M psi15.4 GPa25th stiffest of 1550.54 M psi4.06 M psiBending strength
16,600 psi114.5 MPa41st strongest of 1554,300 psi29,900 psiCupping tendency
1.9062nd highest of 1551.092.90Shrinkage across the face
7.6%radial 4.0%70th lowest of 1553.5%12.7%
For its weight: stiffness-to-weight 2.65 (144th of 155); strength-to-weight 19,762 psi (152nd of 155).
How much it moves
Both its face shrinkage (7.6%) and its T/R ratio (1.90) sit in the middle half of the list.
0.46 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.24 in.
- Tangential
- 7.6%
- Radial
- 4.0%
- Volume
- 10.0%
- T/R ratio
- 1.90 (94th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Piquia
20% softer · 14% lighter · shrinks 0.4 points more across the face
- Courbaril
9% harder · 16% lighter · shrinks 0.9 points more across the face
- Black locust
21% softer · 21% lighter · shrinks 0.4 points less across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Side hardness | 1,910lbf | 2,160lbf | +13% | 9,608N |
| Compression parallel to grain | 6,580psi | 10,320psi | +57% | 71.2MPa |
| Modulus of elasticity | 1.94M psi | 2.23M psi | +15% | 15.4GPa |
| Modulus of rupture | 12,100psi | 16,600psi | +37% | 114.5MPa |
| Shear parallel to grain | 1,760psi | 1,960psi | +11% | 13.5MPa |
| Work to maximum load | 6.70in-lbf/in³ | 10.4in-lbf/in³ | +55% | 71.7kJ/m³ |