Afrormosia
Pericopsis elata
Afrormosia measures 1,560 lbf on the Janka scale, 21% harder than northern red oak.
- It pairs hardness with little movement: harder than 77% of the woods, yet in the lowest quarter for shrinkage across the face.
- Unusually, it tests harder green (1,600 lbf) than dry.
- Across all 155 woods it falls in the top fifth for bending strength and T/R ratio and in the bottom fifth for face shrinkage and radial shrinkage.
U.S. hardwoodsU.S. softwoodsImported woodsNorthern red oak
Six measures
AfrormosiaImported woods medianOther woods
Bending strength
18,400 psi126.9 MPa25th strongest of 1554,300 psi29,900 psiShrinkage across the face
6.4%radial 3.0%29th lowest of 1553.5%12.7%Cupping tendency
2.1331st highest of 1551.092.90Janka hardness
1,560 lbf6,939 N36th hardest of 15530th of 65 imported woods240 lbf3,680 lbfDensity
0.6138th heaviest of 1550.250.96Stiffness
1.94 M psi13.4 GPa44th stiffest of 1550.54 M psi4.06 M psi
For its weight: strength-to-weight 30,164 psi (17th of 155).
How much it moves
Total movement is small, but most of it runs along the rings (T/R 2.13), so a flatsawn board still loses 2.1 times the width of a quartersawn one.
0.38 in.
off a 6-inch flatsawn board, green to oven-dry; quartersawn 0.18 in.
- Tangential
- 6.4%
- Radial
- 3.0%
- Volume
- 10.7%
- T/R ratio
- 2.13 (124th most stable of 155)
End view, shrinkage drawn 3× life size.
Closest substitutes
- Sepetir
10% softer · 8% lighter · shrinks 0.6 points more across the face
- Purpleheart
19% harder · 10% heavier · shrinks 0.3 points less across the face
- Peroba de campos
3% harder · 2% heavier · shrinks 0.2 points more across the face
Woods of similar hardness
The eight nearest on the Janka scale, lbf.
Laboratory values
| Property | Green | Dry, 12% MC | Change when dried | Metric, 12% MC |
|---|---|---|---|---|
| Work to maximum load | 19.5in-lbf/in³ | 18.4in-lbf/in³ | −6% | 126.9kJ/m³ |
| Compression parallel to grain | 7,490psi | 9,940psi | +33% | 68.5MPa |
| Shear parallel to grain | 1,670psi | 2,090psi | +25% | 14.4MPa |
| Modulus of rupture | 14,800psi | 18,400psi | +24% | 126.9MPa |
| Side hardness | 1,600lbf | 1,560lbf | −2% | 6,939N |
| Modulus of elasticity | 1.77M psi | 1.94M psi | +10% | 13.4GPa |
Note on the data: the published side hardness at 12% MC is lower than the green value.
Wood Handbook Table 5-5b, Table 4-4. Data & method · Guides