Douglas-fir
Hardness among the 3 douglas-fir here ranges from 600 lbf (Douglas-fir (Interior North)) to 710 lbf (Douglas-fir (Coast)). The flattest-drying is Douglas-fir (Interior West); the stiffest is Douglas-fir (Coast).
- The hardest is only 1.18 times as hard as the softest, one of the three narrowest spreads among the 15 families here.
- Its median hardness, 660 lbf, is 32% above the median for U.S. softwoods.
- All three sit in the middle half of the 155 woods for hardness, between 565 lbf and 1,465 lbf.
- Density runs from a specific gravity of 0.45 in Douglas-fir (Coast) to 0.46 in Douglas-fir (Interior West).
- 660 lbfmedian hardness
- 0.45median density
- 12,600 psimedian bending strength
- 7.5%median face shrinkage
Douglas-firOther woodsNorthern red oak, the usual yardstick
Ranked by hardness
Hardest first. Density is specific gravity; shrinkage is volumetric, green to oven-dry.
| # | Wood | Janka, lbf | Density | Bending, psi | Shrinkage |
|---|---|---|---|---|---|
| 1 | Douglas-fir (Coast)Pseudotsuga menziesiiSG 0.45 · 12.4% shrinkage | 710 | 0.45 | 12,400 | 12.4% |
| 2 | Douglas-fir (Interior West)Pseudotsuga menziesiiSG 0.46 · 11.8% shrinkage | 660 | 0.46 | 12,600 | 11.8% |
| 3 | Douglas-fir (Interior North)Pseudotsuga menziesiiSG 0.45 · 10.7% shrinkage | 600 | 0.45 | 13,100 | 10.7% |
Source: USDA Forest Products Laboratory, Wood Handbook (2010), Tables 4-3, 4-4, 5-3b and 5-5b. How we use the data · Compare or filter these woods · Guide: Hardwood vs softwood in numbers